Nanoparticle grafted fluorosilane coupling agent compatibilized fluorine / silicone rubber and preparation method thereof
Through nanoparticle grafting fluorosilane coupling agent compatibilization technology, the problem of poor compatibility when blending fluorine rubber and silicone rubber is solved, complementary performance is achieved, and the mechanical and thermal properties of fluorine/silicone rubber composite materials are improved.
Patent Information
- Application Number
- CN202410900024.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
Fluorine rubber and silicone rubber have large compatibility differences when blended, making it difficult to achieve effective cross-linking, resulting in poor complementary performance, especially in terms of low temperature resistance and high strength.
Nanoparticles are grafted with a fluorosilane coupling agent as a compatibilizer. The nanoparticles are modified by preparing a fluorosilane coupling agent and added to the fluorine/silicone rubber. The properties of the nanoparticles are improved through steps such as ultrasonic dispersion, hydrolysis and stirring. Dispersibility and chemical reactivity, enhance the compatibility of fluorine rubber and silicone rubber, and form a three-dimensional network structure through vulcanization treatment to improve performance.
It significantly improves the compatibility of fluorine rubber and silicone rubber, reduces the low-temperature brittleness temperature, and improves the mechanical and thermal properties, making the properties of fluorine rubber and silicone rubber complementary, making up for the shortcomings of a single rubber.
Smart Images

Figure CN118725484A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of rubber composite materials and relates to a nano-particle grafted fluorosilane coupling agent-compatibilized fluorine / silicone rubber and a preparation method thereof. Background Art
[0002] Fluororubber has the characteristics of high temperature resistance, oil resistance, and corrosion resistance. It is an indispensable sealing material for the aerospace, automotive, and shipbuilding industries. The presence of fluorine atoms in fluororubber leads to its high potential energy and molecular rigidity, and its glass transition temperature (Tg) is about -18°C, which limits its application in high-latitude cold areas. In contrast, silicone rubber maintains the elasticity and flexibility of its molecular chain within the temperature range of -70°C to -90°C. However, silicone rubber has poor mechanical properties. A single fluororubber or silicone rubber cannot fully meet the diverse requirements of various applications, especially in terms of low temperature resistance and high strength. Therefore, these two rubbers are used together to produce fluorosilicone rubber or silicone rubber / fluororubber blends that have the advantages of both fluororubber and silicone rubber, so that their performance is complementary to further broaden the application field of rubber.
[0003] However, due to the different chemical structures and physical properties of fluororubber and silicone rubber, their compatibility is poor, and it is difficult to achieve crosslinking between fluororubber and silicone rubber by simply blending them. Nanoparticles have high specific surface area, high surface activity and high interfacial stability, and have attracted widespread attention in the capacity expansion of incompatible blending systems. Compared with traditional compatibilizers, inorganic nanoparticles as compatibilizers have the advantages of small addition amount, wide source, low cost, easy industrialization, ability to regulate polymer phase structure, and giving special functionality to composite materials, and are used in the capacity expansion research of incompatible polymer blending systems. However, the effect of simply adding nanoparticle solubilizers to modify fluorosilicone rubber blending is not ideal, and it is urgent to develop new capacity expansion and modification methods to achieve complementary advantages of fluorosilicone rubber and improve performance. Summary of the invention
[0004] To solve the above problems, the present invention provides a nanoparticle grafted fluorosilane coupling agent to increase the compatibility of fluororubber and silicone rubber and a preparation method thereof, so as to improve the compatibility of fluororubber and silicone rubber and make their performance complementary to each other, so as to further broaden the application field of rubber.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] A nanoparticle grafted fluorosilane coupling agent compatibilized fluorine / silicone rubber comprises the following components in parts by weight: 10-90 parts of fluororubber, 10-90 parts of silicone rubber, 10-40 parts of fluorosilane coupling agent modified nanoparticles, 1-2 parts of vulcanizing agent BIPB, 2-3 parts of vulcanization accelerator TAIC, and 0.2-1 part of hydroxy silicone oil.
[0007] The fluororubber is any one of 26-type fluororubber, 246-type fluororubber, tetrapropylene fluororubber, perfluoroether rubber, and the like.
[0008] The silicone rubber is any one of methyl silicone rubber, methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber and the like.
[0009] The fluorosilane coupling agent modified nanoparticles are prepared by reacting nanoparticles with a fluorosilane coupling agent. The modified nanoparticles are used as nano-compatibilizers and added to fluoro / silicone rubber to prepare a fluoro / silicone rubber composite material with excellent comprehensive performance.
[0010] Another object of the present invention is to provide a method for preparing nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber, the steps comprising:
[0011] The first step is to prepare fluorosilane coupling agent modified nanoparticles:
[0012] S1. Add nanoparticles to an anhydrous ethanol solution at room temperature and ultrasonically disperse for 0.5 to 1 hour to obtain solution A; the nanoparticles are one or more of nano-silicon dioxide, nano-silicon, nano-carbon black, nano-titanium dioxide, carbon nanotubes (CNTs), graphene, etc.
[0013] S2. Disperse the fluorosilane coupling agent in a mixed solution of anhydrous ethanol / deionized water, add sodium hydroxide to adjust the pH value to 5-6, and hydrolyze for 1-2 hours to obtain solution B; the fluorosilane coupling agent is any one or more of trifluoroethylsilane coupling agent, hexafluoropropyltrimethoxysilane coupling agent, trimethoxydodecafluorooctylsilane coupling agent, dimethoxydodecafluorooctylsilane coupling agent, tridecafluorooctyltriethoxysilane, etc.
[0014] S3. The solutions A and B obtained in steps S1 and S2 are mixed evenly, and then stirred in a water bath at 80° C. for 5 to 6 hours; the mass ratio of the nanoparticles in solution A to the fluorosilane coupling agent in solution B is 10:1-10:3.
[0015] S4. Centrifuge the solution obtained in step S3, remove the precipitate, wash it, and dry it at 80° C. for 24 hours to obtain fluorosilane coupling agent-modified nanoparticles.
[0016] The second step is to weigh the fluororubber according to the raw material ratio, plasticize it for 10-20 times, add the nano-compatibilizer, mix it evenly after the material is completely eaten, roll it several times, triangle pack it several times, and place it down to obtain the mixed fluororubber. The number of rolling and triangle packing is more than 5 times.
[0017] The third step is to weigh the silicone rubber according to the raw material ratio, roll it, add hydroxy silicone oil, mix it evenly, and place it on the sheet to obtain the mixed silicone rubber.
[0018] In the fourth step, the mixed fluororubber prepared in the second step is added to the mixed silicone rubber prepared in the third step, and then the vulcanizing agent BIPB and the vulcanization accelerator TAIC are added, and mixed evenly to prepare a fluoro / silicone rubber blend. During the mixing process, the fluororubber and the silicone rubber are mixed evenly.
[0019] The fifth step is to vulcanize the fluorine / silicone rubber blend prepared in the fourth step at a temperature of 160-180°C, a pressure of 15-20 MPa, and a vulcanization time of 5-8 minutes. During the vulcanization process, the linear molecular structure in the fluorine / silicone rubber is converted into a three-dimensional network structure by the action of the vulcanizing agent, thereby significantly improving the physical and chemical properties of the rubber.
[0020] In the sixth step, the fluorine / silicone rubber blend treated in the fifth step is subjected to a second stage vulcanization at a vulcanization temperature of 200-230°C and a vulcanization time of 10-12 hours; the mixture is naturally cooled to room temperature and placed for 8-16 hours to obtain a product. During the vulcanization process, the degree of vulcanization in the rubber can be increased to achieve better mechanical strength and thermal properties.
[0021] The beneficial effects of the present invention are as follows:
[0022] (1) The inorganic nanoparticles in the present invention have a small particle size and contain many chemical functional groups on the surface, such as hydroxyl, carboxyl, amine, etc. A fluorosilane coupling agent is grafted on the surface of the nanoparticles to introduce fluorine atom groups and siloxane groups. The modified nanoparticles have enhanced chemical reactivity and improved dispersibility, and can stably exist on the two-phase interface of fluororubber and silicone rubber, thereby achieving a compatibilization effect and improving the compatibility of fluororubber and silicone rubber.
[0023] (2) The low-temperature brittle temperature and TR10 temperature of the blended rubber of the present invention are greatly reduced, and the mechanical properties are also significantly improved. At the same time, compared with the control group without adding nano-compatibilizer, only adding the same mass of nano-particles, it is found that the nano-compatibilizer has better low-temperature performance and mechanical properties on fluoro / silicone rubber than the control group. The addition of the nano-compatibilizer of the present invention achieves the compatibility of fluororubber and silicone rubber, making up for the performance defects of single fluororubber or silicone rubber.
[0024] (3) The preparation method of the present invention is simple, the conditions are controllable, and it can be prepared on a conventional production line. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope image of the brittle fracture cross section of Example 1. It can be seen from the image that the fluorine / silicone rubber mixture is evenly distributed without obvious phase separation areas. DETAILED DESCRIPTION
[0026] In order to better understand the present invention, the present invention is further described below by way of examples. The examples are only used to explain the present invention and will not constitute any limitation to the present invention.
[0027] Example 1
[0028] Nanoparticles grafted with fluorosilane coupling agent to increase the compatibilization of fluorine / silicone rubber, the raw materials include the following components by mass: 90 parts of fluororubber, 10 parts of silicone rubber, 10 parts of fluorosilane coupling agent modified nanoparticles, 1 part of vulcanizing agent BIPB, 2 parts of vulcanization accelerator TAIC, and 0.2 parts of hydroxy silicone oil. Among them, the fluorosilane coupling agent modified nanoparticles are used as nano-compatibilizers. In this embodiment, the fluororubber is 26 type fluororubber and the silicone rubber is methyl vinyl silicone rubber. The preparation process includes the following steps:
[0029] (1) Weigh fluororubber according to the raw material ratio, plasticize it 10 times, add nano-compatibilizer, and after the material is completely absorbed, mix it evenly, roll it 5 times, triangle pack it 5 times, and place it under the sheet.
[0030] (2) Weigh the silicone rubber according to the raw material ratio, roll it, add hydroxy silicone oil, mix well, and place it on the sheet.
[0031] (3) adding the mixed fluororubber prepared in step (1) to the mixed silicone rubber prepared in step (2), and then adding BIPB and TAIC, mixing evenly to prepare fluoro / silicone rubber.
[0032] (4) The fluorine / silicone rubber blend is subjected to a first stage vulcanization at a vulcanization temperature of 175°C, a pressure of 15 MPa, and a vulcanization time of 6 min.
[0033] (5) The fluorine / silicone rubber blend treated in step (4) is subjected to a second-stage vulcanization at a vulcanization temperature of 200° C. for a vulcanization time of 12 h; the mixture is naturally cooled to room temperature and placed for 16 h.
[0034] In this embodiment 1, in step (1), the nano-compatibilizer is prepared by the following method using nanoparticles and a fluorosilane coupling agent as raw materials:
[0035] S1. Add nanoparticles into anhydrous ethanol solution at room temperature and disperse them by ultrasonic for 0.5 h to obtain solution A; the nanoparticles are nano-silicon dioxide.
[0036] S2. Disperse the fluorosilane coupling agent in a mixed solution of anhydrous ethanol / deionized water, add sodium hydroxide to adjust the pH value to 5, and hydrolyze for 1 hour to obtain solution B; the fluorosilane coupling agent is tridecafluorooctyltriethoxysilane.
[0037] S3. The solutions A and B obtained in steps S1 and S2 are mixed evenly, and then stirred in a water bath at 80° C. for 5 h; the mass ratio of the nanoparticles in solution A to the fluorosilane coupling agent in solution B is 10:3.
[0038] S4. Centrifuge the solution obtained in step S3, remove the precipitate, wash, and dry at 80° C. for 24 hours to obtain fluorosilane coupling agent modified nanoparticles. The modified nanoparticles are added to fluoro / silicone rubber as nanocompatibility enhancers to prepare fluoro / silicone rubber composite materials with excellent comprehensive properties.
[0039] Example 2
[0040] Nanoparticles grafted with fluorosilane coupling agent to increase the compatibilization of fluorine / silicone rubber, the raw materials include the following components by mass: 50 parts of fluororubber, 50 parts of silicone rubber, 40 parts of fluorosilane coupling agent modified nanoparticles, 2 parts of vulcanizing agent BIPB, 3 parts of vulcanization accelerator TAIC, and 0.6 parts of hydroxy silicone oil. Among them, the fluorosilane coupling agent modified nanoparticles are used as nano-compatibilizers. In this embodiment, the fluororubber is tetrapropylene fluororubber and the silicone rubber is methyl vinyl phenyl silicone rubber. The preparation process includes the following steps:
[0041] (1) Weigh fluororubber according to the raw material ratio, plasticize it 20 times, add nano-compatibilizer, and mix evenly after the material is completely eaten, roll it 5 times, triangle pack it 5 times, and place it under the sheet.
[0042] (2) Weigh the silicone rubber according to the raw material ratio, roll it, add hydroxy silicone oil, mix well, and place it on the sheet.
[0043] (3) adding the mixed fluororubber prepared in step (1) to the mixed silicone rubber prepared in step (2), and then adding BIPB and TAIC, mixing evenly to prepare fluoro / silicone rubber.
[0044] (4) The fluorine / silicone rubber blend is subjected to a first stage vulcanization at a vulcanization temperature of 160°C, a pressure of 20 MPa, and a vulcanization time of 8 min.
[0045] (5) The fluorine / silicone rubber blend treated in step (4) was subjected to a second-stage vulcanization at a vulcanization temperature of 215° C. for a vulcanization time of 11 h; the mixture was naturally cooled to room temperature and allowed to stand for 8 h.
[0046] In this embodiment 1, in step (1), the nano-compatibilizer is prepared by the following method using nanoparticles and a fluorosilane coupling agent as raw materials:
[0047] S1. Add nanoparticles into anhydrous ethanol solution at room temperature and disperse them by ultrasonic for 1 hour to obtain solution A; the nanoparticles are nano-titanium dioxide.
[0048] S2. Disperse the fluorosilane coupling agent in a mixed solution of anhydrous ethanol / deionized water, add sodium hydroxide to adjust the pH value to 6, and hydrolyze 1.5 to obtain solution B; the fluorosilane coupling agent is trifluoroethylsilane coupling agent.
[0049] S3. The solutions A and B obtained in steps S1 and S2 are mixed evenly, and then stirred in a water bath at 80° C. for 5.5 h; the mass ratio of the nanoparticles in solution A to the fluorosilane coupling agent in solution B is 10:2.
[0050] S4. Centrifuge the solution obtained in step S3, remove the precipitate, wash, and dry at 80° C. for 24 hours to obtain fluorosilane coupling agent modified nanoparticles. The modified nanoparticles are added to fluoro / silicone rubber as nanocompatibility enhancers to prepare fluoro / silicone rubber composite materials with excellent comprehensive properties.
[0051] Example 3
[0052] Nanoparticles grafted with fluorosilane coupling agent to increase the compatibilization of fluorine / silicone rubber, the raw materials include the following components by mass: 10 parts of fluororubber, 90 parts of silicone rubber, 25 parts of fluorosilane coupling agent modified nanoparticles, 1.5 parts of vulcanizing agent BIPB, 2.5 parts of vulcanization accelerator TAIC, and 1 part of hydroxy silicone oil. Among them, the fluorosilane coupling agent modified nanoparticles are used as nano-compatibility agents. In this embodiment, the fluororubber is parafluoroether rubber and the silicone rubber is methyl silicone rubber. The preparation process includes the following steps:
[0053] (1) Weigh fluororubber according to the raw material ratio, plasticize it 15 times, add nano-compatibilizer, and after the material is completely absorbed, mix it evenly, roll it 5 times, triangle pack it 5 times, and place it on the lower sheet.
[0054] (2) Weigh the silicone rubber according to the raw material ratio, roll it, add hydroxy silicone oil, mix well, and place it on the sheet.
[0055] (3) adding the mixed fluororubber prepared in step (1) to the mixed silicone rubber prepared in step (2), and then adding BIPB and TAIC, mixing evenly to prepare fluoro / silicone rubber.
[0056] (4) The fluorine / silicone rubber blend is subjected to a first stage vulcanization at a vulcanization temperature of 180°C, a pressure of 18 MPa, and a vulcanization time of 5 min.
[0057] (5) The fluorine / silicone rubber blend treated in step (4) is subjected to a second-stage vulcanization at a vulcanization temperature of 230° C. for a vulcanization time of 10 h; the mixture is naturally cooled to room temperature and allowed to stand for 12 h.
[0058] In this embodiment 1, in step (1), the nano-compatibilizer is prepared by the following method using nanoparticles and a fluorosilane coupling agent as raw materials:
[0059] S1. Add nanoparticles into anhydrous ethanol solution at room temperature and disperse them by ultrasonic for 0.8 h to obtain solution A; the nanoparticles are CNTs.
[0060] S2. Disperse the fluorosilane coupling agent in a mixed solution of anhydrous ethanol / deionized water, add sodium hydroxide to adjust the pH value to 5.5, and hydrolyze for 2 hours to obtain solution B; the fluorosilane coupling agent is trimethoxy dodecafluorooctylsilane coupling agent.
[0061] S3. The solutions A and B obtained in steps S1 and S2 are mixed evenly, and then stirred in a water bath at 80° C. for 6 hours; the mass ratio of the nanoparticles in solution A to the fluorosilane coupling agent in solution B is 10:1.
[0062] S4. Centrifuge the solution obtained in step S3, remove the precipitate, wash, and dry at 80° C. for 24 hours to obtain fluorosilane coupling agent modified nanoparticles. The modified nanoparticles are added to fluoro / silicone rubber as nanocompatibility enhancers to prepare fluoro / silicone rubber composite materials with excellent comprehensive properties.
[0063] Comparative Example 1
[0064] The difference from Example 1 is that no nano-compatibilizer is added, only the same mass fraction of nano-particles are added, and the other components and processes remain unchanged. The prepared fluoro / silicone rubber is subjected to performance testing in the same manner as in Example 1.
[0065] The properties of the prepared fluoro / silicone rubber were tested according to the test method (the tensile test was in accordance with GB / T 528-2009; the low temperature brittleness test was in accordance with GB / T 1682-2014; the low temperature shrinkage test was in accordance with GB / T 7758-2002), and the results are as follows:
[0066]
[0067] From the data analysis of Table 1, it can be seen that the addition of nano-compatibilizer can effectively improve the compatibility of fluororubber and silicone rubber, so that the low temperature resistance of silicone rubber and the strengthening and toughening effect of nanoparticles can be fully exerted. Compared with comparative example 1, the tensile strength is increased by 4.6MPa, the elongation at break is increased by 60%, the brittle temperature is reduced by -10℃, and TR10 is reduced by 7℃.
[0068] The above descriptions are embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related fields, are also included in the patent protection scope of the present invention.
Claims
1. A nanoparticle grafted fluorosilane coupling agent to increase the compatibilization of fluorine / silicone rubber, characterized in that: The nanoparticle grafted fluorosilane coupling agent compatibilized fluoro / silicone rubber comprises the following components in parts by weight: 10-90 parts of fluororubber, 10-90 parts of silicone rubber, 10-40 parts of fluorosilane coupling agent modified nanoparticles, 1-2 parts of vulcanizing agent, 2-3 parts of vulcanization accelerator, and 0.2-1 part of hydroxy silicone oil.
2. The nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 1, characterized in that: The fluororubber is any one of 26-type fluororubber, 246-type fluororubber, tetrapropylene fluororubber, parafluoroether rubber and perfluoroether rubber.
3. The nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 1, characterized in that: The silicone rubber is any one of methyl silicone rubber, methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber and the like.
4. The nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 1, characterized in that: The fluorosilane coupling agent modified nanoparticles are prepared from nanoparticles and fluorosilane coupling agents.
5. A method for preparing the nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to any one of claims 1 to 4, characterized in that: The following steps are involved: In the first step, nanoparticles and fluorosilane coupling agent are used as raw materials to prepare fluorosilane coupling agent-modified nanoparticles as nanocompatibility enhancers; The second step is to weigh the fluororubber according to the raw material ratio, plasticize it for 10-20 times, add the nano-compatibilizer, and mix it evenly after the material is completely eaten to obtain the mixed fluororubber; The third step is to weigh the silicone rubber according to the raw material ratio, roll it, add hydroxy silicone oil, mix it evenly, and obtain the mixed silicone rubber; The fourth step is to add the mixed fluororubber prepared in the second step to the mixed silicone rubber prepared in the third step, and then add the vulcanizing agent BIPB and the vulcanization accelerator TAIC, mix them evenly, and prepare a fluoro / silicone rubber blend; The fifth step is to subject the fluorine / silicone rubber blend prepared in the fourth step to a stage of vulcanization; In the sixth step, the fluorine / silicone rubber blend treated in the fifth step is subjected to a second-stage vulcanization, and then naturally cooled to room temperature and left to stand for a certain period of time to obtain a product.
6. The method for preparing nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 5, characterized in that: The specific steps of the first step are as follows: S1. adding the nanoparticles to an anhydrous ethanol solution at room temperature, and obtaining solution A after ultrasonic dispersion; S2. Disperse the fluorosilane coupling agent in a mixed solution of anhydrous ethanol / deionized water, add sodium hydroxide to adjust the pH value to 5-6, and hydrolyze for 1-2 hours to obtain solution B; S3. The solutions A and B obtained in steps S1 and S2 are mixed evenly, and then stirred in a water bath at 80° C. for 5 to 6 hours; the mass ratio of the nanoparticles in solution A to the fluorosilane coupling agent in solution B is 10:1-10:3; S4. Centrifuge the solution obtained in step S3, remove the lower precipitate, and dry it to obtain fluorosilane coupling agent modified nanoparticles.
7. The method for preparing nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 6, characterized in that: The nanoparticles are one or more of nano-silicon dioxide, nano-silicon, nano-carbon black, nano-titanium dioxide, carbon nanotubes, and graphene; the fluorosilane coupling agent is any one or more of trifluoroethylsilane coupling agent, hexafluoropropyltrimethoxysilane coupling agent, trimethoxydodecafluorooctylsilane coupling agent, dimethoxydodecafluorooctylsilane coupling agent, tridecafluorooctyltriethoxysilane, and the like.
8. The method for preparing nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 5, characterized in that: The temperature of the first stage vulcanization in the fifth step is 160-180° C., the pressure is 15-20 MPa, and the vulcanization time is 5-8 minutes.
9. The method for preparing nanoparticle-grafted fluorosilane coupling agent-compatibilized fluoro / silicone rubber according to claim 5, characterized in that: The temperature of the second stage vulcanization in the sixth step is 200-230° C., the vulcanization time is 10-12 hours, and the placement time is 8-16 hours.
Citation Information
Cited By
Modified perfluoroether rubber as well as preparation method and application thereof
CN120484412A
Static sealing material and preparation process thereof
CN120554864A
High-temperature-resistant fluororubber sheathed cable capable of being vulcanized and bonded and preparation method thereof
CN121617746A
Low-temperature modifier, preparation method thereof and application of low-temperature modifier in hydrogen energy sealing fluororubber
CN121914314A