A durable brake pad
Through the combination of phenolic resin/carbon fiber composite and other materials, the durability and heat attenuation of brake pads after high temperature friction is solved, and the brake pads with high friction coefficient, low noise, low wear and low cost are achieved, taking into account environmental protection Sexual and economical.
Patent Information
- Application Number
- CN202411233038.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The existing brake pads have insufficient durability, heat attenuation, unstable friction coefficient, noise problems and environmental protection problems after high-temperature friction, making it difficult to ensure high performance while taking into account the feasibility of cost control and large-scale production.
Using phenolic resin/carbon fiber composite as core components, a complex network structure is formed through carbon fiber pretreatment, acid chloride and polyphenylene sulfide grafting, combined with barite powder, boron nitride powder, polypropylene mesh fiber, glass Fiber and bentonite are used to prepare brake pads using low-cost processes to improve their heat resistance, thermal conductivity and stability.
It significantly improves the heat resistance and wear resistance of the brake pads, extends the service life, reduces noise and manufacturing costs, takes into account environmental protection and economicality, and ensures excellent performance under high temperature, high speed and emergency braking conditions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction materials, and in particular to a durable brake pad. Background Art
[0002] Brake pads are key components in the automotive braking system. Their main function is to slow down or stop the movement of the vehicle through friction with the brake disc or brake drum. Generally speaking, brake pads are composed of steel plates, adhesive insulation layers and friction blocks. Among them, the friction blocks are composed of friction materials and adhesives. During the braking process, they are squeezed on the brake disc or brake drum to generate friction, thereby achieving the purpose of slowing down or stopping the vehicle.
[0003] Friction material is the core determinant of brake pad performance. It is usually made by ordinary hot pressing of synthetic materials at a temperature below 200°C. The raw materials of friction material mainly include four parts:
[0004] Binder: usually phenolic resin, which affects the thermal decay performance, recovery performance, wear performance and mechanical properties of the material. Reinforcement fiber: acts as a reinforcing agent. Traditional materials use mineral fibers such as asbestos, while semi-metallic brake pads mainly use steel fibers, and a small amount of copper fibers and mineral fibers are added. Friction performance regulator: divided into two categories: friction-reducing materials (such as graphite, molybdenum disulfide, lead and copper, etc.) and friction materials, used to adjust the friction coefficient and improve wear resistance. Filler: mainly added in the form of powder.
[0005] The main indicators for measuring brake pad performance include: Friction coefficient: determines the basic braking torque and needs to be within an appropriate range to avoid wheel locking or excessive braking distance. Safety: pays special attention to performance under high temperature conditions. Comfort: includes braking feel, noise, dust, smoke and odor, etc. Service life: usually requires a service life of 30,000 kilometers.
[0006] However, existing brake pads still have some problems: Insufficient durability: Ordinary phenolic resins have the disadvantages of poor thermal ablation and high wear, and are prone to physical and chemical changes during emergency braking and high-speed braking, resulting in a reduced brake pad life. Thermal attenuation phenomenon: Brake pads that use asbestos as reinforcing fibers have poor thermal conductivity, which can easily cause heat accumulation, affect braking performance, and even cause brake failure. Unstable friction coefficient: The use of steel fibers and iron fibers in semi-metallic brake pads may result in an unstable friction coefficient. Noise problem: Some brake pads will produce harsh noises during use, affecting the driving experience. Environmental issues: Some brake pad materials contain ingredients that are harmful to the environment, such as asbestos and heavy metals.
[0007] Chinese patent document CN118440460A discloses a durable and long-life brake pad and a preparation method thereof. The brake pad is made of the following components, measured by weight: 10 to 20 parts of modified phenolic resin, 6 to 12 parts of rubber powder, 2 to 8 parts of antigorite, 1 to 5 parts of magnesium oxide, 1 to 9 parts of aluminum oxide, 1 to 5 parts of silicon carbide, 3 to 9 parts of flake graphite, 2 to 8 parts of carbon black, 2 to 8 parts of bentonite, 8 to 16 parts of modified carbon fiber, 4 to 10 parts of aramid fiber, and 2 to 6 parts of ceramic fiber.
[0008] Researchers have been exploring new materials and processes to improve the overall performance of brake pads. However, how to ensure the high performance of brake pads while taking into account cost control and the feasibility of large-scale production remains the focus and difficulty of current research. Therefore, developing a brake pad that can simultaneously meet the requirements of durability, stability, environmental protection and economy has important practical significance and market value. Summary of the invention
[0009] In order to address the deficiencies in the prior art, the purpose of the present invention is to provide a durable brake pad which has a good surface condition and no decomposition after high-temperature friction, effectively avoids thermal decay, and exhibits excellent thermal stability and durability, while taking into account both environmental protection and economy, using environmentally friendly materials and low-cost processes, maintaining market competitiveness while protecting the environment, and is expected to become an ideal choice for automotive braking systems.
[0010] In order to achieve the above object, the present invention adopts the following technical solution:
[0011] A durable brake pad is made of the following components by weight: 15-25 parts of phenolic resin / carbon fiber composite, 10-15 parts of barite powder, 5-12 parts of boron nitride powder, 3-8 parts of polypropylene mesh fiber, 1-6 parts of glass fiber, 1-5 parts of rubber powder, and 0.5-3 parts of bentonite.
[0012] Preferably, the barite particle size is 500-700 mesh.
[0013] Preferably, the boron nitride has a particle size of 300-500 mesh and is hexagonal boron nitride.
[0014] Preferably, the rubber powder has a particle size of 40-60 meshes, a Mooney viscosity of 90-140 at 100° C., a combined acrylonitrile content of 37-40%, a gel content of 70-90%, and a volatile matter ≤1.0%.
[0015] Preferably, the method for preparing the phenolic resin / carbon fiber composite comprises the following steps:
[0016] Carbon fiber surface pretreatment and modification: First, concentrated nitric acid oxidizes the carbon fiber surface to introduce hydroxyl and carboxyl groups. Subsequently, a silane coupling agent (3-[3-carboxyallylamide]propyltriethoxysilane) reacts with the carbon fiber surface hydroxyl groups to form Si-OC covalent bonds and introduce carboxyl groups and double bonds. This step increases the activity and functional group density of the carbon fiber surface.
[0017] (1) Soaking the carbon fiber in concentrated sulfuric acid, taking it out and washing it with deionized water, then adding it to anhydrous ethanol, and then adding 3-[3-carboxyallylamide]propyltriethoxysilane, stirring and mixing, filtering, washing and drying the product to obtain pretreated carbon fiber;
[0018] Preferably, in step (1), the concentration of concentrated sulfuric acid is 95-98 wt % and the soaking time is 30-60 min.
[0019] Preferably, in step (1), the amount ratio of carbon fiber, anhydrous ethanol and 3-[3-carboxyallylamide]propyltriethoxysilane is 10 g:100 mL:0.5-3 g; and the stirring and mixing conditions are stirring and mixing at 30-60° C. for 2-4 hours.
[0020] Acid chloride treatment: Sulfonyl chloride (SOCl2) reacts with the carboxyl groups on the carbon fiber surface to convert them into acyl chloride groups. The reaction mechanism involves nucleophilic addition of carboxyl groups to SOCl2, followed by removal of SO2 and HCl to form acyl chloride. This step increases the surface reactivity and prepares for subsequent polymer grafting.
[0021] (2) adding the pretreated carbon fiber and thionyl chloride into anhydrous dichloromethane, reflux reacting in a fume hood, washing the product with anhydrous dichloromethane, and drying to obtain chlorinated carbon fiber;
[0022] Preferably, in step (2), the usage ratio of pretreated carbon fiber, thionyl chloride and anhydrous dichloromethane is 10 g: 4-8 g: 50-100 mL.
[0023] Preferably, in step (2), the reflux reaction conditions are 40-50° C. for 2-5 h.
[0024] Polyphenylene sulfide grafting: The polyphenylene sulfide containing thiol groups at the end undergoes a nucleophilic substitution reaction with the acyl chloride groups on the surface of the carbon fiber. As a nucleophilic reagent, the thiol group attacks the carbon atom of the acyl chloride to form an ester bond and releases HCl (neutralized by triethylamine). This step covalently grafts polyphenylene sulfide to the surface of the carbon fiber, enhancing the interfacial compatibility.
[0025] (3) Adding chlorinated carbon fiber and polyphenylene sulfide into DMF, uniformly dispersing by ultrasonication, continuously introducing nitrogen, then dropping triethylamine, stirring for reaction, washing the product with acetone, and drying, to obtain polyphenylene sulfide grafted carbon fiber;
[0026] Preferably, in step (3), the number average molecular weight of the polyphenylene sulfide is 4000-5000.
[0027] Preferably, in step (3), the usage ratio of chlorinated carbon fiber, polyphenylene sulfide and triethylamine is 10 g: 3-8 g: 0.1-1 mL.
[0028] Preferably, in step (3), the stirring reaction condition is 60-80° C. for 4-6 hours.
[0029] Final modification: Benzoyl peroxide (BPO) thermally decomposes to produce free radicals, which initiate free radical polymerization and crosslinking reactions between allyl phenolic resin, sodium dithiosuccinate and residual double bonds on the surface of carbon fiber. This step forms a complex three-dimensional network structure, further improving the degree of modification and interface bonding strength of the carbon fiber surface.
[0030] (4) Add polyphenylene sulfide grafted carbon fiber, allyl phenolic resin, and sodium dithiosuccinate to acetone, disperse them evenly by ultrasonication, continuously introduce nitrogen, add BPO dropwise, heat and react, wash the product with acetone and deionized water, and dry to obtain a phenolic resin / carbon fiber composite.
[0031] Preferably, in step (4), the usage ratio of polyphenylene sulfide grafted carbon fiber, allyl phenolic resin, sodium dithiosuccinate, and BPO is 10 g: 30-60 g: 2-6 g: 0.1-1 g.
[0032] Preferably, in step (4), the temperature reaction is carried out at 70-90° C. for 4-7 hours.
[0033] The present invention also claims protection for a method for preparing the durable brake pad, comprising the following steps: adding phenolic resin / carbon fiber composite, barite powder, boron nitride powder, polypropylene mesh fiber, glass fiber, rubber powder, and bentonite into a mixer and mixing evenly to obtain a mixture; adding the mixture into a press and pressing at 30-35 MPa and 150-160°C for 30-45 minutes to obtain a semi-finished product; heat treating the semi-finished product at 170-180°C for 5-8 hours, and chamfering, coarse grinding, and fine grinding to obtain the durable brake pad.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1) The present invention provides a durable brake pad, which uses a phenolic resin / carbon fiber composite as a core component, greatly improving the heat resistance and wear resistance of the brake pad. The addition of barite powder and boron nitride powder improves the thermal conductivity and effectively alleviates the thermal attenuation phenomenon. The addition of polypropylene mesh fibers enhances the bonding strength between the fibers and the friction material and improves the overall structural stability. Bentonite, as a friction-reducing material, can not only absorb friction heat, but also reduce the hardness and noise of the material. Rubber particles can reduce vibration, absorb noise of a certain wavelength, and at the same time buffer the impact force generated during braking to prevent the surface of the friction material from heating up too quickly. The prepared brake pad has the comprehensive advantages of high friction coefficient, low noise, low wear, high porosity and low manufacturing cost. Under extreme conditions such as high temperature, high speed and emergency braking, the brake pad of the present invention can still maintain excellent performance, significantly extend the service life, and take into account environmental protection and economy.
[0036] 2) The present invention provides a method for preparing a phenolic resin / carbon fiber composite, firstly, pretreating the carbon fiber to increase its surface activity. Subsequently, active groups are introduced through an acyl chloride reaction to prepare for the subsequent grafting reaction. Next, a grafting reaction of polyphenylene sulfide is carried out, wherein the thiol group at the end of the polyphenylene sulfide undergoes a substitution reaction with the active chlorine in the acyl chloride carbon fiber to form a polyphenylene sulfide grafted carbon fiber. This step significantly improves the compatibility of the carbon fiber with the resin and introduces a rigid and regular crystal structure. Finally, the allyl phenolic resin is combined with the modified carbon fiber through a free radical polymerization reaction to form a composite material with a network structure. This series of reactions ensures a strong interfacial interaction between the carbon fiber and the resin matrix, thereby significantly improving the overall performance of the composite material.
[0037] 3) The present invention provides a phenolic resin / carbon fiber composite, in which a chemical bond is formed between the carbon fiber and the resin matrix, which greatly enhances the interfacial bonding strength and improves the overall mechanical properties and wear resistance of the material. The introduction of polyphenylene sulfide not only improves the heat resistance and chemical stability of the composite, but the alternating arrangement of benzene rings and sulfur atoms in its molecular chain further enhances the mechanical strength of the brake pad. Moreover, the formation of the network structure improves the thermal conductivity and thermal stability of the composite, effectively alleviates the problem of thermal attenuation, and expands the high-temperature braking range. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0039] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0040] The carbon fiber was T700 chopped carbon fiber purchased from Tianniao High-Tech Co., Ltd.
[0041] The glass fiber is 3~6mm alkali-free glass fiber purchased from Tongxiang Jushi Group Co., Ltd.
[0042] A method for preparing a durable brake pad comprises the following steps:
[0043] (1) Soak 10 g of carbon fiber in 50 mL of 95-98 wt% concentrated sulfuric acid for 30-60 min, take it out and wash it with deionized water, then add it to 100 mL of anhydrous ethanol, then add 0.5-3 g of 3-[3-carboxyallylamide]propyltriethoxysilane, stir and mix at 30-60 ° C for 2-4 h, filter, wash and dry the product to obtain pretreated carbon fiber;
[0044] (2) Add 10 g of pretreated carbon fiber and 4-8 g of thionyl chloride to 50-100 mL of anhydrous dichloromethane, reflux for 2-5 h at 40-50 °C in a fume hood, wash the product with anhydrous dichloromethane and dry it to obtain chlorinated carbon fiber;
[0045] (3) Add 10 g of chlorinated carbon fiber and 3-8 g of polyphenylene sulfide into 100 mL of DMF, disperse them evenly by ultrasonication, continuously introduce nitrogen, then drop 0.1-1 mL of triethylamine, stir and react at 60-80 °C for 4-6 h, wash the product with acetone and dry it to obtain polyphenylene sulfide grafted carbon fiber;
[0046] (4) Add 10 g of polyphenylene sulfide grafted carbon fiber, 30-60 g of allyl phenolic resin, and 2-6 g of sodium dithiosuccinate to acetone, disperse them uniformly by ultrasonication, continuously introduce nitrogen, add 0.1-1 g of BPO dropwise, react at 70-90 °C for 4-7 h, wash the product with acetone and deionized water, and dry it to obtain a phenolic resin / carbon fiber composite;
[0047] (5) Add 15-25 parts of phenolic resin / carbon fiber composite, 10-15 parts of barite powder, 5-12 parts of boron nitride powder, 3-8 parts of polypropylene mesh fiber, 1-6 parts of glass fiber, 1-5 parts of rubber powder, and 0.5-3 parts of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 30-35 MPa and 150-160° C. for 30-45 minutes to obtain a semi-finished product; heat treat the semi-finished product at 170-180° C. for 5-8 hours, and obtain the durable brake pad by chamfering, coarse grinding, and fine grinding.
[0048] The present invention will be further described below through specific embodiments.
[0049] Example 1
[0050] A method for preparing a durable brake pad comprises the following steps:
[0051] (1) 10 g of carbon fiber was soaked in 50 mL of 98 wt% concentrated sulfuric acid for 60 min, taken out and washed with deionized water, then added to 100 mL of anhydrous ethanol, and then 3 g of 3-[3-carboxyallylamide]propyltriethoxysilane was added, and the mixture was stirred and mixed at 60 ° C for 2 h. The product was filtered, washed, and dried to obtain pretreated carbon fiber;
[0052] (2) Add 10 g of pretreated carbon fiber and 8 g of thionyl chloride to 100 mL of anhydrous dichloromethane, reflux for 2 h at 50 °C in a fume hood, wash the product with anhydrous dichloromethane and dry it to obtain chlorinated carbon fiber;
[0053] (3) Add 10 g of chlorinated carbon fiber and 8 g of polyphenylene sulfide into 100 mL of DMF, disperse them evenly by ultrasonication, continuously introduce nitrogen, then drop 1 mL of triethylamine, stir and react at 80 °C for 4 h, wash the product with acetone and dry it to obtain polyphenylene sulfide grafted carbon fiber;
[0054] (4) 10 g of polyphenylene sulfide grafted carbon fiber, 60 g of allyl phenolic resin, and 6 g of sodium dithiosuccinate were added to acetone, ultrasonically dispersed evenly, nitrogen was continuously introduced, 1 g of BPO was added dropwise, and the reaction was carried out at 90 ° C for 4 h. The product was washed with acetone and deionized water, and dried to obtain a phenolic resin / carbon fiber composite;
[0055] (5) Add 25 kg of phenolic resin / carbon fiber composite, 15 kg of barite powder, 12 kg of boron nitride powder, 8 kg of polypropylene mesh fiber, 6 kg of glass fiber, 5 kg of rubber powder, and 3 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the durable brake pad by chamfering, rough grinding, and fine grinding.
[0056] Example 2
[0057] A method for preparing a durable brake pad comprises the following steps:
[0058] (1) Soak 10 g of carbon fiber in 50 mL of 95-98 wt% concentrated sulfuric acid for 30-60 min, take it out and wash it with deionized water, then add it to 100 mL of anhydrous ethanol, then add 0.5-3 g of 3-[3-carboxyallylamide]propyltriethoxysilane, stir and mix at 30-60 ° C for 2-4 h, filter, wash and dry the product to obtain pretreated carbon fiber;
[0059] (2) Add 10 g of pretreated carbon fiber and 4-8 g of thionyl chloride to 50-100 mL of anhydrous dichloromethane, reflux for 2-5 h at 40-50 °C in a fume hood, wash the product with anhydrous dichloromethane and dry it to obtain chlorinated carbon fiber;
[0060] (3) Add 10 g of chlorinated carbon fiber and 6 g of polyphenylene sulfide into 100 mL of DMF, disperse them evenly by ultrasonication, continuously introduce nitrogen, then dropwise add 0.8 mL of triethylamine, stir and react at 75 °C for 5 h, wash the product with acetone and dry it to obtain polyphenylene sulfide grafted carbon fiber;
[0061] (4) 10 g of polyphenylene sulfide grafted carbon fiber, 50 g of allyl phenolic resin, and 5 g of sodium dithiosuccinate were added to acetone, ultrasonically dispersed evenly, nitrogen was continuously introduced, 0.6 g of BPO was added dropwise, and the reaction was carried out at 85 °C for 5 h. The product was washed with acetone and deionized water, and dried to obtain a phenolic resin / carbon fiber composite;
[0062] (5) Add 22 kg of phenolic resin / carbon fiber composite, 14 kg of barite powder, 10 kg of boron nitride powder, 6 kg of polypropylene mesh fiber, 5 kg of glass fiber, 4 kg of rubber powder, and 2.5 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the durable brake pad by chamfering, rough grinding, and fine grinding.
[0063] Example 3
[0064] A method for preparing a durable brake pad comprises the following steps:
[0065] (1) 10 g of carbon fiber was soaked in 50 mL of 98 wt% concentrated sulfuric acid for 60 min, taken out and washed with deionized water, then added to 100 mL of anhydrous ethanol, and then 1 g of 3-[3-carboxyallylamide]propyltriethoxysilane was added, and the mixture was stirred and mixed at 40 ° C for 3 h. The product was filtered, washed, and dried to obtain pretreated carbon fiber;
[0066] (2) Add 10 g of pretreated carbon fiber and 5 g of thionyl chloride to 100 mL of anhydrous dichloromethane, reflux for 4 h at 44 °C in a fume hood, wash the product with anhydrous dichloromethane and dry it to obtain chlorinated carbon fiber;
[0067] (3) Add 10 g of chlorinated carbon fiber and 5 g of polyphenylene sulfide into 100 mL of DMF, disperse them evenly by ultrasonication, continuously introduce nitrogen, then drop 0.4 mL of triethylamine, stir and react at 70 °C for 5 h, wash the product with acetone and dry it to obtain polyphenylene sulfide grafted carbon fiber;
[0068] (4) 10 g of polyphenylene sulfide grafted carbon fiber, 40 g of allyl phenolic resin, and 3 g of sodium dithiosuccinate were added to acetone, ultrasonically dispersed evenly, nitrogen was continuously introduced, 0.4 g of BPO was added dropwise, and the reaction was carried out at 80 ° C for 5 h. The product was washed with acetone and deionized water, and dried to obtain a phenolic resin / carbon fiber composite;
[0069] (5) Add 18 kg of phenolic resin / carbon fiber composite, 13 kg of barite powder, 8 kg of boron nitride powder, 5 kg of polypropylene mesh fiber, 3 kg of glass fiber, 2 kg of rubber powder, and 2 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the durable brake pad by chamfering, rough grinding, and fine grinding.
[0070] Example 4
[0071] A method for preparing a durable brake pad comprises the following steps:
[0072] (1) 10 g of carbon fiber was soaked in 50 mL of 98 wt% concentrated sulfuric acid for 60 min, taken out and washed with deionized water, then added to 100 mL of anhydrous ethanol, and then 0.5 g of 3-[3-carboxyallylamide]propyltriethoxysilane was added, and the mixture was stirred and mixed at 30 ° C for 4 h. The product was filtered, washed, and dried to obtain pretreated carbon fiber;
[0073] (2) Add 10 g of pretreated carbon fiber and 4 g of thionyl chloride to 100 mL of anhydrous dichloromethane, reflux for 5 h at 40 °C in a fume hood, wash the product with anhydrous dichloromethane and dry it to obtain chlorinated carbon fiber;
[0074] (3) Add 10 g of chlorinated carbon fiber and 3 g of polyphenylene sulfide into 100 mL of DMF, disperse them evenly by ultrasonication, continuously introduce nitrogen, then drop 0.1 mL of triethylamine, stir and react at 60 °C for 6 h, wash the product with acetone and dry it to obtain polyphenylene sulfide grafted carbon fiber;
[0075] (4) 10 g of polyphenylene sulfide grafted carbon fiber, 30 g of allyl phenolic resin, and 2 g of sodium dithiosuccinate were added to acetone, ultrasonically dispersed evenly, nitrogen was continuously introduced, 0.1 g of BPO was added dropwise, and the reaction was carried out at 70 ° C for 7 h. The product was washed with acetone and deionized water, and dried to obtain a phenolic resin / carbon fiber composite;
[0076] (5) Add 15 kg of phenolic resin / carbon fiber composite, 10 kg of barite powder, 5 kg of boron nitride powder, 3 kg of polypropylene mesh fiber, 1 kg of glass fiber, 1 kg of rubber powder, and 0.5 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the durable brake pad by chamfering, coarse grinding, and fine grinding.
[0077] Comparative Example 1
[0078] A method for preparing a brake pad comprises the following steps:
[0079] (1) 10 g of carbon fiber was soaked in 50 mL of 98 wt% concentrated sulfuric acid for 60 min, taken out and washed with deionized water, then added to 100 mL of anhydrous ethanol, and then 3 g of 3-[3-carboxyallylamide]propyltriethoxysilane was added, and the mixture was stirred and mixed at 60 ° C for 2 h. The product was filtered, washed, and dried to obtain pretreated carbon fiber;
[0080] (2) 10 g of pretreated carbon fiber, 60 g of allyl phenolic resin, and 6 g of sodium dithiosuccinate were added to acetone, ultrasonically dispersed evenly, nitrogen was continuously introduced, 1 g of BPO was added dropwise, and the reaction was carried out at 90 °C for 4 h. The product was washed with acetone and deionized water, and dried to obtain a phenolic resin / carbon fiber composite;
[0081] (3) Add 25 kg of phenolic resin / carbon fiber composite, 15 kg of barite powder, 12 kg of boron nitride powder, 8 kg of polypropylene mesh fiber, 6 kg of glass fiber, 5 kg of rubber powder, and 3 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the brake pad by chamfering, rough grinding, and fine grinding.
[0082] Comparative Example 2
[0083] A method for preparing a brake pad comprises the following steps:
[0084] (1) 10 g of carbon fiber was soaked in 50 mL of 98 wt% concentrated sulfuric acid for 60 min, taken out and washed with deionized water, then added to 100 mL of anhydrous ethanol, and then 3 g of 3-[3-carboxyallylamide]propyltriethoxysilane was added, and the mixture was stirred and mixed at 60 ° C for 2 h. The product was filtered, washed, and dried to obtain pretreated carbon fiber;
[0085] (2) Add 20 kg of allyl phenolic resin, 5 kg of pretreated carbon fiber, 15 kg of barite powder, 12 kg of boron nitride powder, 8 kg of polypropylene mesh fiber, 6 kg of glass fiber, 5 kg of rubber powder, and 3 kg of bentonite into a mixer and mix evenly to obtain a mixture; add the mixture into a press and press at 32 MPa and 155° C. for 40 min to obtain a semi-finished product; heat treat the semi-finished product at 175° C. for 7 h, and obtain the brake pad by chamfering, rough grinding, and fine grinding.
[0086] The performance tests were carried out on the brake pads prepared in Examples 1 to 4 and Comparative Examples 1 to 2. The Rockwell hardness of the brake pads was tested using an XHR-150 plastic Rockwell hardness tester with reference to GB / T 5766-2023 "Test method for Rockwell hardness of friction materials". The impact strength test was carried out using a simply supported beam pendulum impact tester with reference to GB / T 1043.2-2018 "Determination of impact properties of plastics - Part 2: Instrumented impact test" (impact energy of 0.98 J and 3.92 J at two levels, and impact speed of 2.9 m / s). The friction coefficient and wear rate were tested using an XD-MSM fixed speed friction tester with reference to GB 5763-2018 "Automobile brake linings" (temperature 200°C, disc speed 480 r / min, clamping force 0.98 MPa). The sound absorption coefficient was measured using an AWA6128A standing wave tube sound absorption coefficient tester. The specific data are shown in Table 1.
[0087] Table 1 Brake pad performance test results
[0088]
[0089] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A durable brake pad, characterized in that: The invention is made of the following components by weight: 15-25 parts of phenolic resin / carbon fiber composite, 10-15 parts of barite powder, 5-12 parts of boron nitride powder, 3-8 parts of polypropylene mesh fiber, 1-6 parts of glass fiber, 1-5 parts of rubber powder, and 0.5-3 parts of bentonite; The preparation method of the phenolic resin / carbon fiber composite comprises the following steps: (1) Soaking the carbon fiber in concentrated sulfuric acid, taking it out and washing it with deionized water, then adding it to anhydrous ethanol, and then adding 3-[3-carboxyallylamide]propyltriethoxysilane, stirring and mixing, filtering, washing and drying the product to obtain pretreated carbon fiber; (2) adding the pretreated carbon fiber and thionyl chloride into anhydrous dichloromethane, reflux reacting in a fume hood, washing the product with anhydrous dichloromethane, and drying to obtain chlorinated carbon fiber; (3) Adding chlorinated carbon fiber and polyphenylene sulfide into DMF, uniformly dispersing by ultrasonication, continuously introducing nitrogen, then dropping triethylamine, stirring for reaction, washing the product with acetone, and drying, to obtain polyphenylene sulfide grafted carbon fiber; (4) Add polyphenylene sulfide grafted carbon fiber, allyl phenolic resin, and sodium dithiosuccinate to acetone, disperse them evenly by ultrasonication, continuously introduce nitrogen, add BPO dropwise, heat and react, wash the product with acetone and deionized water, and dry to obtain a phenolic resin / carbon fiber composite.
2. The brake pad according to claim 1, characterized in that: In step (1), the concentration of concentrated sulfuric acid is 95-98 wt %; the soaking time is 30-60 min; the amount ratio of carbon fiber, anhydrous ethanol, and 3-[3-carboxyallylamide]propyltriethoxysilane is 10 g:100 mL:0.5-3 g; and the stirring and mixing conditions are stirring and mixing at 30-60 ° C for 2-4 h.
3. The brake pad according to claim 1, characterized in that: In step (2), the usage ratio of pretreated carbon fiber, thionyl chloride and anhydrous dichloromethane is 10 g: 4-8 g: 50-100 mL.
4. The brake pad according to claim 1, characterized in that: In step (2), the reflux reaction conditions are 40-50° C. for 2-5 h.
5. The brake pad according to claim 1, characterized in that: In step (3), the usage ratio of chlorinated carbon fiber, polyphenylene sulfide and triethylamine is 10 g: 3-8 g: 0.1-1 mL.
6. The brake pad according to claim 1, characterized in that: In step (3), the stirring reaction conditions are 60-80° C. for 4-6 hours.
7. The brake pad according to claim 1, characterized in that: In step (4), the usage ratio of polyphenylene sulfide grafted carbon fiber, allyl phenolic resin, sodium dithiosuccinate and BPO is 10g:30~60g:2~6g:0.1~1g.
8. The brake pad according to claim 1, characterized in that: In step (4), the temperature of the reaction is 70-90° C. for 4-7 hours.
9. A method for preparing a durable brake pad as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding phenolic resin / carbon fiber composite, barite powder, boron nitride powder, polypropylene mesh fiber, glass fiber, rubber powder and bentonite into a mixer and mixing them evenly to obtain a mixture; adding the mixture into a press and pressing the mixture at 30-35MPa and 150-160°C for 30-45min to obtain a semi-finished product; heat treating the semi-finished product at 170-180°C for 5-8h, chamfering, coarse grinding and fine grinding to obtain the durable brake pad.