Aspartame polyurea transparent waterproof coating with high elastic recovery rate and preparation method and application thereof
By using specific components to react in asparagus polyurea transparent waterproof coatings to form urea bond structures, the elastic recovery rate and adhesion of the coating are improved, and the problem of decreased adhesion at the tiles joints in the prior art is solved, and the cooling is achieved High adhesion effect in thermal environment.
Patent Information
- Application Number
- CN202411230047.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The elastic recovery rate and adhesion of the existing aspen polyurea transparent waterproof coatings at the tiles are insufficient, and they cannot meet the use requirements in the alternating environment of hot and cold, resulting in the problem of decreased adhesion and shedding.
High elastic recovery rate asparagus polyurea transparent waterproof coating prepared by reacting component A and component B at a mass ratio of 1: (1-3). Component A contains polyaspartic acid ester resin, defoaming agent, and moisturizing. Wetting agent, leveling agent, UV absorber and antioxidant, component B forms an urea bond structure through reaction of aliphatic diisocyanate, modified polytetrahydrofuran ether glycol and monounitous end amino polyether to increase the elastic modulus of the coating and low temperature flexibility.
The elastic recovery rate and adhesion of the paint are improved, and the adhesion of >90% can be maintained in hot and cold environments, meeting the deformation needs of tiles, and solving the problem of difficulty in maintaining adhesion in the prior art.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waterproof coatings, and in particular relates to an aspartame polyurea transparent waterproof coating with a high elastic recovery rate, and a preparation method and application thereof. Background Art
[0002] Asparagus polyurea waterproof coating can be used on the base surface of ceramic tiles. It can not only repair the ceramic tile joints, but also fill the ceramic tile joints. It has the effect of plugging leaks and increasing the life of the overall waterproof layer. The material used as ceramic tile joint filler must have a strong elastic recovery ability, otherwise, after the joint shrinks, the joint filler will be higher than the road surface, and will be squeezed and rubbed by external forces for a long time, reducing its life. At the same time, the joint filler must have a certain hardness to avoid the embedding of hard objects and the loss of expansion and contraction function of the joint.
[0003] However, most of the existing transparent waterproof coatings for tile base surfaces do not meet the requirement of >300% elongation at break, and do not meet the standard of TCWA204-2021 polyaspartic acid waterproof coating. Even if the standard is met, the elastic recovery rate is poor. At the same time, the expansion and contraction caused by the alternating hot and cold environment leads to the adhesion retention rate at the tile joints failing to meet the standard, resulting in large-scale peeling and peeling after a period of use.
[0004] Chinese invention patent application publication number CN107474712A discloses a high-strength aspartic polyurea waterproof coating and a preparation method thereof, which discloses the use of aspartic acid ester in combination with high-solid, low-viscosity elastic polyurethane-type isocyanate to enhance the softness, wear resistance and adhesion of the coating film. However, the resilience is insufficient and cannot solve the problem of decreased adhesion of the tile waterproof coating caused by deformation of tile joints due to alternating hot and cold temperatures.
[0005] China Invention Patent Application Publication No. CN115895421A A transparent solvent-free tile waterproof coating, preparation method and application, discloses that the curing agent obtained by compounding HT-600, GB930-100, HT400, TolonateTMXF450 and HDI prepolymer has a lower viscosity, and the waterproof coating compounded with low-activity polyaspartic acid ester has a longer application period, slower reaction activity, and is transparent. However, the physical and mechanical properties of the paint film are relatively poor, and do not meet the TCWA204-2021 polyaspartic acid ester waterproof coating standard. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a transparent waterproof coating of aspartame with high elastic recovery rate, which has high elongation and elastic recovery rate and maintains good adhesion in cold and hot environments. The present invention also provides a preparation method and application thereof.
[0007] The asparagus polyurea transparent waterproof coating with high elastic recovery rate of the present invention is prepared by reacting component A and component B in a mass ratio of 1:(1-3);
[0008] Component A is composed of the following raw materials in parts by weight: 91-95 parts of polyaspartic acid ester resin, 0.1-0.3 parts of defoaming agent, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of leveling agent, 1-2 parts of ultraviolet absorber, 1-2 parts of antioxidant, and 1-6 parts of silane coupling agent; the number average molecular weight of the polyaspartic acid ester resin is 550-665;
[0009] Component B is composed of the following raw materials in parts by weight: 29-43 parts of aliphatic diisocyanate, 52-64 parts of modified polytetramethylene ether diol, and 5-11.5 parts of monofunctional amino-terminated polyether, wherein the monofunctional amino-terminated polyether is a polyether monoamine having only one terminal amino functional group in its molecular structure.
[0010] Preferably, the polyaspartic acid ester resin is one of TD420, TD421 and TD422 produced by Shandong Century United New Material Technology Co., Ltd.
[0011] Preferably, the aliphatic diisocyanate is one or more of isophorone diisocyanate, hexamethylene diisocyanate or 4,4'-dicyclohexylmethane diisocyanate.
[0012] Preferably, the preparation method of the modified polytetrahydrofuran ether diol is as follows: isophorone diamine, polytetrahydrofuran ether diol and tetrabutyl titanate catalyst are added into a reactor, nitrogen is replaced under normal temperature, the temperature is raised to 130-150°C and the temperature is maintained constant, the pressure in the reactor is pumped down to -0.1MPa, and then ethylene oxide is added for polymerization reaction, and after the addition is completed, the reaction is carried out at 100-120°C for 1h to obtain the modified polytetrahydrofuran ether diol. In a low temperature environment, the modified polytetrahydrofuran ether diol can also flow normally, and the melting point is reduced from the original 15-35°C to 0-15°C, providing better low temperature performance.
[0013] Preferably, in parts by weight, isophorone diamine is 5-10 parts, polytetramethylene ether diol is 82-88 parts, tetrabutyl titanate is 0.1-0.3 parts, and ethylene oxide is 6.9-10 parts; the number average molecular weight of polytetramethylene ether diol is 650.
[0014] Preferably, the monofunctional amino polyether is one or both of ZFL-1001 and FL-1000.
[0015] The method for preparing the asparagine polyurea transparent waterproof coating with high elastic recovery rate of the present invention comprises the following steps:
[0016] (1) Add the modified polytetramethylene glycol to the reactor, vacuum dehydrate it, add aliphatic diisocyanate at 35-45°C, heat it up for reaction, then add monofunctional amino polyether for end-capping reaction, cool it down to stop the reaction, and obtain component B;
[0017] (2) The raw material of component A and component B are mixed evenly in a mass ratio of 1:(1-3) to obtain the asparagine polyurea transparent waterproof coating with high elastic recovery rate.
[0018] Preferably, in step (1), the temperature of the temperature-raising reaction is 95-110° C., and the reaction time is 5-6 h.
[0019] Preferably, in step (1), the temperature of the end-capping reaction is 110-130° C., and the reaction time is 1-2 h.
[0020] Application of the aspartame polyurea transparent waterproof coating with high elastic recovery rate on a ceramic tile base surface.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention uses a prepolymer formed by the reaction of aliphatic isocyanate and a heat-resistant and cold-resistant polyol-modified polytetramethylene glycol with a high elastic modulus, and then uses a monofunctional amino polyether to terminate part of the isocyanate to form a prepolymer with a urea bond structure, which further improves the overall elastic modulus and can better adapt to the hot and cold deformation of tile joints, thereby improving the adhesion at the tile joints; the modified polytetramethylene glycol has better low-temperature flexibility, lower melting point, and better elastic modulus, so that the prepolymer formed by the reaction has a good elastic recovery rate, better adapts to the deformation of tile joints and maintains adhesion;
[0023] 2. The present invention solves the problem of adhesion of existing tile waterproof transparent coatings on smooth surfaces. In particular, when the elongation is greater than 300%, the elastic recovery rate can be maintained at more than 90%, which better solves the problem of difficulty in maintaining adhesion of tile joints in a cold and hot shrinkage environment;
[0024] 3. The preparation method of the present invention has simple process, convenient operation, scientific and reasonable, and efficient production. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0026] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0027] Some of the raw materials used in the examples and comparative examples are described as follows:
[0028] TD420, TD421, TD422, polyaspartic acid ester resin, Shandong Century United New Material Technology Co., Ltd.;
[0029] NH1420, number average molecular weight 560, Covestro Polymers (China) Co., Ltd.;
[0030] ZFL-1001, monofunctional amino-terminated polyether a, Zibo Zhengda Polyurethane Co., Ltd.;
[0031] FL-1000, monofunctional amino-terminated polyether b, Changde New Materials Technology Co., Ltd.;
[0032] FL-1000, monofunctional amino-terminated polyether c, Zhejiang Royal Madrid Technology Co., Ltd.;
[0033] Defoamer 2685, Guangzhou Efka Sodium Additive Co., Ltd.;
[0034] Wetting agent 3254, Guangzhou Efka Sodium Additive Co., Ltd.;
[0035] Leveling agent 5066, Guangzhou Efka Sodium Additive Co., Ltd.;
[0036] UV absorber B90, BASF (China) Technology Co., Ltd.;
[0037] Antioxidant 1010, BASF (China) Technology Co., Ltd.;
[0038] Silane coupling agent KH-560, Shandong Sike New Materials Co., Ltd.
[0039] Example 1
[0040] The asparagine polyurea transparent waterproof coating with high elastic recovery rate is prepared by reacting component A and component B in a mass ratio of 1:1;
[0041] Component A is composed of the following raw materials in parts by weight: 91 parts of polyaspartic acid ester resin TD420 (number average molecular weight is 550), 0.1 parts of defoamer 2685, 0.5 parts of wetting agent 3254, 0.1 parts of leveling agent 5066, 2 parts of ultraviolet absorber B90, 1 part of antioxidant 1010, and 5.3 parts of silane coupling agent KH-560.
[0042] Component B is composed of the following raw materials in parts by weight: 43 parts of isophorone diisocyanate, 52 parts of modified polytetramethylene ether diol, and 5 parts of ZFL-1001 (monofunctional amino polyether a).
[0043] Preparation method of modified polytetrahydrofuran ether diol:
[0044] In terms of weight parts, 5 parts of isophorone diamine, 88 parts of polytetramethylene oxide with a number average molecular weight of 650 and 0.1 parts of tetrabutyl titanate catalyst are put into a reactor. After nitrogen replacement under room temperature, the temperature is raised to 130°C and maintained at a constant temperature. The reactor is stirred and dehydrated for 2 hours. The pressure in the reactor is pumped to -0.1 MPa, and then 6.9 parts of ethylene oxide are added to carry out polymerization reaction. After the addition is completed, the reaction is carried out at 100°C for 1 hour to obtain modified polytetramethylene oxide.
[0045] The preparation method of the aspartame polyurea transparent waterproof coating with high elastic recovery rate comprises the following steps:
[0046] (1) Add modified polytetramethylene glycol to the reactor, vacuum dehydrate for 2 hours, add isophorone diisocyanate at 35°C, heat to react for 5 hours, and then add ZFL-1001 (monofunctional amino polyether a), react at 110°C for 2 hours, cool down, filter and fill to obtain component B;
[0047] (2) Component A and component B are mixed evenly in a mass ratio of 1:1 to obtain an asparagine polyurea transparent waterproof coating with a high elastic recovery rate.
[0048] Example 2
[0049] The asparagine polyurea transparent waterproof coating with high elastic recovery rate is prepared by reacting component A and component B in a mass ratio of 1:2;
[0050] Component A is composed of the following raw materials in parts by weight: 93 parts of polyaspartic acid ester resin TD421 (number average molecular weight is 610), 0.2 parts of defoamer 2685, 0.2 parts of wetting agent 3254, 0.2 parts of leveling agent 5066, 1 part of ultraviolet absorber B90, 1 part of antioxidant 1010, and 4.4 parts of silane coupling agent KH-560.
[0051] Component B is composed of the following raw materials in parts by weight: 27 parts of isophorone diisocyanate, 4.5 parts of hexamethylene diisocyanate, 58.5 parts of modified polytetramethylene ether diol, and 10 parts of FL-1000 (monofunctional amino polyether b).
[0052] Preparation method of modified polytetrahydrofuran ether diol:
[0053] In parts by weight, 10 parts of isophorone diamine, 82 parts of polytetramethylene oxide diol with a number average molecular weight of 650 and 0.2 parts of tetrabutyl titanate as catalyst are put into a reaction kettle. After nitrogen replacement at room temperature, the temperature is raised to 140°C and maintained at a constant temperature. The mixture is stirred and dehydrated for 2 hours. The pressure in the reaction kettle is pumped to -0.1MPa, and then 7.8 parts of ethylene oxide are added for polymerization reaction. After the addition is completed, the reaction is carried out at 110°C for 1 hour to obtain the product.
[0054] The preparation method of the aspartame polyurea transparent waterproof coating with high elastic recovery rate comprises the following steps:
[0055] (1) Add modified polytetramethylene ether diol into the reactor, vacuum dehydrate for 2 hours, add isophorone diisocyanate and hexamethylene diisocyanate at 40°C, heat to react for 6 hours, and then add FL-1000 (monofunctional amino polyether b), react at 120°C for 2 hours, cool down, filter and fill to obtain component B;
[0056] (2) Component A and component B are mixed evenly in a mass ratio of 1:2 to obtain an asparagus polyurea transparent waterproof coating with a high elastic recovery rate.
[0057] Example 3
[0058] The asparagus polyurea transparent waterproof coating with high elastic recovery rate is prepared by reacting component A and component B in a mass ratio of 1:3;
[0059] Component A is composed of the following raw materials in parts by weight: 95 parts of polyaspartic acid ester resin TD422 (number average molecular weight is 665), 0.3 parts of defoamer 2685, 0.1 parts of wetting agent 3254, 0.5 parts of leveling agent 5066, 1.1 parts of ultraviolet absorber B90, 2 parts of antioxidant 1010, and 1 part of silane coupling agent KH-560.
[0060] Component B is composed of the following raw materials in parts by weight: 2 parts of isophorone diisocyanate, 29 parts of 4,4'-dicyclohexylmethane diisocyanate, 57.5 parts of modified polytetramethylene ether diol, 5 parts of FL-1000 (monofunctional amino polyether b), and 6.5 parts of ZFL-1001 (monofunctional amino polyether a).
[0061] Preparation method of modified polytetrahydrofuran ether diol:
[0062] In terms of weight, 7 parts of isophorone diamine, 82.7 parts of polytetramethylene oxide diol with a number average molecular weight of 650 and 0.3 parts of tetrabutyl titanate catalyst are put into a reactor. After nitrogen replacement at room temperature, the temperature is raised to 150°C and maintained at a constant temperature. The reactor is stirred and dehydrated for 2 hours. The pressure in the reactor is pumped to -0.1MPa, and then 10 parts of ethylene oxide are added for polymerization reaction. After the addition is completed, the reaction is carried out at 120°C for 1 hour to obtain the product.
[0063] The preparation method of the aspartame polyurea transparent waterproof coating with high elastic recovery rate comprises the following steps:
[0064] (1) Add modified polytetramethylene glycol to the reactor, vacuum dehydrate for 2 hours, add isophorone diisocyanate and 4,4'-dicyclohexylmethane diisocyanate at 45°C, heat to react for 5.5 hours, and then add FL-1000 (monofunctional amino polyether b) and ZFL-1001 (monofunctional amino polyether a), and react at 130°C for 2 hours. Cool down, filter and fill to obtain component B;
[0065] (2) Component A and component B are mixed evenly in a mass ratio of 1:3 to obtain an asparagine polyurea transparent waterproof coating with a high elastic recovery rate.
[0066] Example 4
[0067] The asparagine polyurea transparent waterproof coating with high elastic recovery rate is prepared by reacting component A and component B in a mass ratio of 1:2;
[0068] Component A is composed of the following raw materials in parts by weight: 91 parts of polyaspartic acid ester resin TD421 (number average molecular weight is 610), 0.2 parts of defoamer 2685, 0.2 parts of wetting agent 3254, 0.2 parts of leveling agent 5066, 1.2 parts of ultraviolet absorber B90, 1.2 parts of antioxidant 1010, and 6 parts of silane coupling agent KH-560.
[0069] Component B is composed of the following raw materials in parts by weight: 29 parts of hexamethylene diisocyanate, 64 parts of modified polytetramethylene ether diol, and 7 parts of FL-1000 (monofunctional amino polyether c).
[0070] Preparation method of modified polytetrahydrofuran ether diol:
[0071] In parts by weight, 6 parts of isophorone diamine, 85 parts of polytetramethylene oxide diol with a number average molecular weight of 650 and 0.2 parts of tetrabutyl titanate catalyst are put into a reactor. After nitrogen replacement at room temperature, the temperature is raised to 145°C and maintained at a constant temperature. The reactor is stirred and dehydrated for 2 hours. The pressure in the reactor is pumped to -0.1MPa, and then 8.8 parts of ethylene oxide are added to carry out polymerization reaction. After the addition is completed, the reaction is carried out at 110°C for 1 hour to obtain the product.
[0072] The preparation method of the aspartame polyurea transparent waterproof coating with high elastic recovery rate comprises the following steps:
[0073] (1) Add modified polytetramethylene ether diol into the reactor, vacuum dehydrate for 2 hours, add hexamethylene diisocyanate at 40°C, heat to react for 6 hours, and then add FL-1000 (monofunctional amino polyether c), react at 130°C for 2 hours, cool down, filter and fill to obtain component B;
[0074] (2) Component A and component B are mixed evenly in a mass ratio of 1:2 to obtain an asparagus polyurea transparent waterproof coating with a high elastic recovery rate.
[0075] Comparative Example 1
[0076] The difference from Example 1 is that the polyaspartic acid ester in component A is replaced by an equal amount of NH1420 with a number average molecular weight of 560, and the rest is the same as Example 1.
[0077] Comparative Example 2
[0078] The difference from Example 3 is that component B is replaced with a commercially available isocyanate curing agent, Asahi Kasei E420-90T elastic curing agent, of equal mass, and the rest is the same as Example 3.
[0079] Comparative Example 3
[0080] The difference from Example 2 is that the modified polytetramethylene ether diol of component B is replaced by unmodified polytetramethylene ether diol with a number average molecular weight of 650, and the rest is the same as Example 2.
[0081] The performance tests of the aspartame polyurea transparent waterproof coatings with high elastic recovery rates prepared in Examples 1-4 and Comparative Examples 1-3 were respectively carried out. The test methods referred to the standard of TCWA204-2021 polyaspartic acid ester waterproof coatings, and the elastic recovery rate was in accordance with the provisions of "JG / T 471 Elastic Sealant for Insulating Glass for Building Doors, Windows and Curtain Walls".
[0082] The test results are shown in Table 1:
[0083] Table 1 Performance test table of Examples 1-4 and Comparative Examples 1-3
[0084]
[0085] As can be seen from Table 1, the asparagine polyurea transparent waterproof coating with high elastic recovery rate prepared in the embodiment meets the standard of TCWA204-2021 polyaspartic acid ester waterproof coating, and the elastic recovery rate meets the standard of "JG / T 471 Insulating glass elastic sealant for building doors, windows and curtain walls". The elastic recovery rate of the asparagine polyurea transparent waterproof coating prepared in Comparative Example 1 is insufficient, and the tensile strength and elastic recovery rate of the asparagine polyurea transparent waterproof coating prepared in Comparative Example 2 are insufficient. The elastic recovery rate of the asparagine polyurea transparent waterproof coating prepared in Comparative Example 3 is insufficient, and the elastic recovery rate decreases significantly after aging.
Claims
1. A transparent waterproof coating of aspartame with high elastic recovery rate, characterized in that: Prepared by reacting component A and component B in a mass ratio of 1:(1-3); Component A is composed of the following raw materials in parts by weight: 91-95 parts of polyaspartic acid ester resin, 0.1-0.3 parts of defoaming agent, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of leveling agent, 1-2 parts of ultraviolet absorber, 1-2 parts of antioxidant, and 1-6 parts of silane coupling agent; the number average molecular weight of the polyaspartic acid ester resin is 550-665; Component B is composed of the following raw materials in parts by weight: 29-43 parts of aliphatic diisocyanate, 52-64 parts of modified polytetramethylene ether diol, and 5-11.5 parts of monofunctional amino polyether; Preparation method of component B: add modified polytetramethylene glycol to a reactor, add aliphatic diisocyanate after vacuum dehydration, heat up for reaction, then add monofunctional amino polyether for end-capping reaction, cool down to stop the reaction, and obtain component B; The preparation method of modified polytetramethylene oxide ether diol is as follows: isophorone diamine, polytetramethylene oxide ether diol and tetrabutyl titanate catalyst are put into a reactor, and after nitrogen replacement under room temperature, the temperature is raised to 130-150°C and maintained at a constant temperature, and the mixture is stirred and dehydrated for 2 hours. The pressure in the reactor is reduced to -0.1MPa, and then ethylene oxide is added for polymerization reaction. After the addition is completed, the mixture is reacted at 100-120°C for 1 hour to obtain the modified polytetramethylene oxide ether diol.
2. The asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 1, characterized in that: The polyaspartic acid ester resin is one of TD420, TD421 and TD422.
3. The asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 1, characterized in that: The aliphatic diisocyanate is one or more of isophorone diisocyanate, hexamethylene diisocyanate or 4,4'-dicyclohexylmethane diisocyanate.
4. The asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 1, characterized in that: In parts by weight, isophorone diamine is 5-10 parts, polytetramethylene ether diol is 82-88 parts, tetrabutyl titanate is 0.1-0.3 parts, and ethylene oxide is 6.9-10 parts; the number average molecular weight of polytetramethylene ether diol is 650.
5. The asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 1, characterized in that: The monofunctional amino polyether is one or both of ZFL-1001 and FL-1000.
6. A method for preparing the aspartame polyurea transparent waterproof coating with high elastic recovery rate according to any one of claims 1 to 5, characterized in that: The steps include: (1) Add the modified polytetramethylene glycol to a reactor, add aliphatic diisocyanate after vacuum dehydration, heat up to react, then add monofunctional amino polyether to cap the reaction, cool down to stop the reaction, and obtain component B; (2) The raw material of component A and component B are mixed evenly in a mass ratio of 1:(1-3) to obtain the asparagine polyurea transparent waterproof coating with high elastic recovery rate.
7. The method for preparing the asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 6, characterized in that: In step (1), the temperature of the temperature-raising reaction is 95-110° C., and the reaction time is 5-6 h.
8. The method for preparing the asparagine polyurea transparent waterproof coating with high elastic recovery rate according to claim 6, characterized in that: In step (1), the temperature of the end-capping reaction is 110-130° C., and the reaction time is 1-2 h.
9. An application of the aspartame polyurea transparent waterproof coating with high elastic recovery rate according to any one of claims 1 to 5, characterized in that: For use on tiled surfaces.