Method for improving corrosion resistance of aluminide cladding coating
By using a combination of solid phase cladding powder and liquid phase binder and modifier in the laser cladding process, a thicker aluminide coating is formed, which solves the problem of aluminum coating thickness and bonding strength in the existing technology. This has significantly improved the corrosion resistance and service life of thermal power pipelines.
Patent Information
- Application Number
- CN202410975830.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The aluminum coating prepared by the existing laser cladding process is thin and has weak bonding force with the substrate, resulting in a short service life of thermal power pipelines, making it difficult to meet the needs of long-term use and reduction of thermal power costs.
By mixing solid-phase cladding powder with liquid-phase binder, spraying to form a pre-sprayed layer, and performing laser cladding processing in an inert atmosphere to form a thicker aluminide cladding coating, using NiAl, Si and Components such as Pt improve the corrosion resistance and metallurgical bonding strength of the coating.
It significantly improves the corrosion resistance and metallurgical bonding strength of the aluminide cladding coating, extends the service life of the pipe, and significantly improves the oxidation resistance in high-temperature water vapor environments.
Smart Images

Figure CN118726971A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material surface alloying and coating preparation, and specifically relates to a method for improving the corrosion resistance of an aluminide cladding coating. Background Art
[0002] Laser cladding technology is a new type of surface modification technology that emerged in the 1970s with the development of high-power lasers. It refers to a surface strengthening method in which alloy powder or ceramic powder and the substrate surface are rapidly heated and melted under the action of a laser beam, and a metallurgically bonded surface coating is formed on the substrate surface after cooling, thereby significantly improving the wear resistance, corrosion resistance, oxidation resistance and other properties of the substrate surface.
[0003] Laser cladding technology has the advantages of fast cooling speed, low coating dilution rate, small part distortion, etc., and the coating produced by it has the characteristics of uniform and dense structure and strong bonding with the substrate, so it is widely used in the preparation of coating materials. In particular, laser cladding technology has almost no restrictions on powder selection, so various metal powders can be used to meet the use requirements.
[0004] Al powder as a coating material has high corrosion resistance, which makes the corrosion resistance of aluminum profile powder coating better than traditional coatings, and can effectively protect the surface of aluminum profiles from corrosion by various corrosive substances such as acid, alkali, salt, oil, etc. Secondly, the hardness of aluminum profile powder coating is higher than that of traditional coatings, which can effectively improve the strength and wear resistance of the aluminum profile surface. Furthermore, aluminum profile powder coating does not contain organic solvents, does not produce volatile organic compounds, and meets environmental protection requirements.
[0005] In the current laser cladding process, most of the metal powders are clad on the workpiece surface simultaneously. The Al coating prepared is thin, only a few microns or tens of microns, and the bonding force between the coating and the substrate is weak. The service life of the pipe can be appropriately improved in the early stage of use, but with the continuous erosion of soot and water vapor, the coating will still fall off and the coating quality is poor. Therefore, in order to improve the corrosion resistance of the coating, it is urgent to further improve this coating to meet the requirements of long-term use of pipelines and reduce thermal power costs. Summary of the invention
[0006] The present disclosure aims to solve at least one of the technical problems of short service life of existing thermal power pipelines and limited service life of aluminum coatings, and to provide a method for improving the corrosion resistance of aluminide cladding coatings.
[0007] The present invention discloses a method for improving the corrosion resistance of an aluminide cladding coating.
[0008] Methods include:
[0009] The solid phase cladding powder and the liquid phase binder are mixed, stirred and ball milled to obtain a cladding slurry;
[0010] Clean and preheat the surface of the workpiece to be plated;
[0011] Spraying the cladding slurry onto the surface of the workpiece to be plated, drying and curing the workpiece to form a pre-sprayed layer on the workpiece surface;
[0012] The workpiece with the pre-sprayed layer is placed in an inert atmosphere for laser cladding treatment, and an aluminide cladding coating is obtained after cooling.
[0013] Optionally, the solid phase cladding powder includes an aluminum infiltration source, a modifier and an activator.
[0014] Optionally, the aluminum diffusion sources are NiAl and Al.
[0015] Optionally, the modifiers are Si and Pt.
[0016] Optionally, the activating agent is NH4Cl.
[0017] Optionally, the content of NiAl is 50-70%;
[0018] The content of Al is 15-40%;
[0019] The content of Si is 0-5%;
[0020] The content of Pt is 0-5%;
[0021] The content of NH4Cl is 0-5%.
[0022] Optionally, the liquid binder is any one of ethyl acetate, polyvinyl alcohol, sodium carboxymethyl cellulose, and nitrocellulose.
[0023] Optionally, the content of the liquid phase binder is 10-30% of the mass of the solid phase cladding powder.
[0024] Optionally, in the laser cladding process, the laser power is 2-2.8 KW, the scanning rate is 20-40 mm / s, the spot diameter is 2-5 mm, the workpiece rotation speed is 0-5 r / min, and the Ar gas flow rate is 15-20 L / min.
[0025] Optionally, the thickness of the spray coating is 1-5 mm;
[0026] The thickness of the aluminide cladding coating is 1.15-2.95 mm.
[0027] The present disclosure proposes a method for improving the corrosion resistance of an aluminide cladding coating, the method comprising: mixing a solid-phase cladding powder and a liquid-phase binder, stirring and ball-milling to obtain a cladding slurry; cleaning and preheating the surface of the workpiece to be plated; spraying the cladding slurry onto the surface of the workpiece to be plated, drying and curing to form a pre-sprayed layer on the workpiece surface; placing the workpiece with the pre-sprayed layer under an inert atmosphere for laser cladding treatment, and obtaining an aluminide cladding coating after cooling. The present disclosure first mixes a solid-phase cladding powder and a liquid-phase binder, sprays them onto the workpiece surface, and then uses a laser cladding process to prepare a thicker coating, effectively increasing the corrosion resistance of the coating. The process has high repeatability and is extremely practical and universal. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A flowchart of a method for improving the corrosion resistance of an aluminide cladding coating according to an embodiment of the present disclosure;
[0029] Figure 2 is a cross-sectional morphology diagram of the aluminide cladding coating in Example 4 of the present disclosure; wherein, Figure 2 (A) is the cross-sectional morphology of the coating; Figure 2 (B) is a partial enlarged view of (A). DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.
[0031] like Figure 1 As shown, the present disclosure proposes a method S100 for improving the corrosion resistance of an aluminide cladding coating, comprising the following specific steps S110 to S140:
[0032] S110, mixing the solid-phase cladding powder and the liquid-phase binder, stirring and ball-milling to obtain a cladding slurry.
[0033] Specifically, each component in the solid-phase cladding powder is sieved through a 1000-mesh screen, and then each component is placed in a planetary ball mill for ball milling and mixing, the ball milling speed is 350-400 rpm, and the time is 12-24 hours. After that, the mixed solid-phase cladding powder is mixed with a liquid-phase binder, and after being fully stirred for 2-4 hours, it is placed in a planetary ball mill for ball milling and mixing, and the ball milling speed is 350-400 rpm and the time is 8-12 hours to obtain a cladding slurry. In other words, the solid-phase cladding powder is first ball milled and pre-mixed, and then the solid-phase cladding powder and the liquid-phase binder are ball milled.
[0034] In some preferred embodiments, the solid phase cladding powder is an aluminum infiltration source, a modifier and an activator. Of course, the total percentage content of each component in the solid phase cladding powder is 100%.
[0035] As a further preferred solution, the aluminum infiltration sources are NiAl and Al, and in terms of mass percentage, the content of NiAl is 50-70%, and the content of Al is 15-40%. For example, the content of NiAl is preferably 50%, 55%, 60%, 65%, 70%, and the content of Al is preferably 15%, 20%, 25%, 30%, 35%, 40%.
[0036] In this embodiment, NiAl is used as one of the components of the aluminum diffusion source, which can form an active intermediate AlCl with NH4Cl. x , thereby promoting the generation of active aluminum atoms and the speed of infiltration into the matrix. Secondly, this component can also be directly clad into the infiltration layer to improve the wear resistance and corrosion resistance of the infiltration layer. Furthermore, this component can also inhibit the generation of brittle aluminum-rich phases such as NiAl3 and Ni2Al3 in the infiltration layer, thereby enhancing the wear resistance of the coating and extending the service life of the pipe.
[0037] As a further preferred solution, the modifier is Si and Pt, wherein, by mass percentage, the content of Si is 0-5%, and the content of Pt is preferably 0-5%. That is to say, in some preferred embodiments, the solid phase cladding powder may not include a modifier, may only include Si components, may only include Pt components, and of course, may also include both Si and Pt components.
[0038] As a further preferred embodiment, the Si content is preferably 1%, 2%, 3%, 4%, and 5%, and the Pt content is preferably 1%, 2%, 3%, 4%, and 5%.
[0039] In this embodiment, the solid phase cladding powder not only contains metal powder, but also contains modifying elements, wherein the addition of modifying element Si can form a continuous SiO2 passivation film, thereby improving the oxidation resistance and heat corrosion resistance. The addition of modifying element Pt can provide a channel for Al element to form a dense oxide, inhibit or reduce the external diffusion of alloy elements, accelerate the transformation of θ-Al2O3 to α-Al2O3, improve the film-base bonding, effectively inhibit internal oxidation and internal sulfidation, and improve the heat corrosion resistance of the coating.
[0040] As a further preferred solution, the activator is NH4Cl, and the content of NH4Cl is 0-5% by mass, for example, 1%, 2%, 3%, 4%, 5%. That is to say, in some preferred embodiments, the solid phase cladding powder may not include an activator.
[0041] It should be understood that when the halide NH4Cl is added to the solid phase cladding powder, this component can play a role in promoting infiltration and activation, thereby improving the infiltration rate and coating quality.
[0042] In other preferred embodiments, the liquid phase binder is ethyl acetate. Of course, the liquid phase binder can also be other high temperature organic binders, such as polyvinyl alcohol, sodium carboxymethyl cellulose aqueous solution, nitrocellulose binder, etc. This liquid phase binder component can make the metal powder into slurry and adhere it to the surface of the substrate, and form a more uniform and dense coating layer after drying and curing; at the same time, it can also prevent the metal powders from bonding to each other to form metal sintered materials, resulting in uneven infiltration layers; moreover, other liquid phase binders such as ethyl acetate volatilize during the laser cladding process and will not affect the process.
[0043] As a further preferred solution, the content of the liquid phase binder is 10-30% of the mass of the solid phase cladding powder, for example, 10%, 15%, 20%, 25%, 30%.
[0044] S120, cleaning and preheating the surface of the workpiece to be plated.
[0045] Specifically, the workpiece to be plated is cleaned with a high-pressure water gun for 5-10 minutes to remove oil stains, dust, etc. on the surface of the workpiece and remove the oxide scale. At the same time, the workpiece can be rinsed with alcohol or acetone to provide a clean and metallic surface for subsequent slurry spraying. After that, the workpiece is preheated at 200-250℃ for 30-60 minutes.
[0046] S130, spraying the cladding slurry onto the surface of the workpiece to be plated, drying and curing the slurry, and forming a pre-sprayed layer on the surface of the workpiece.
[0047] Specifically, the cladding slurry obtained in step S110 is sprayed once onto the surface of the workpiece after the treatment in step S120, and naturally air-dried for 24-48 hours. Thereafter, it is cured at 300-450°C for 24-48 hours to obtain a pre-sprayed layer on the surface of the workpiece. The thickness of the pre-sprayed layer is 1-5 mm, and the coating coverage is not less than 98%. If the slurry layer is too thin, it is insufficient to provide sufficient infiltration source, and if it is too thick, it is easy to crack and peel off, affecting the uniformity of the infiltration layer thickness.
[0048] It should be understood that in this embodiment, the slurry is sprayed to a suitable thickness at one time and cannot be sprayed in layers multiple times.
[0049] In this embodiment, the segmented slurry curing process of natural air drying combined with low-temperature curing is adopted to effectively avoid the problem of micro cracks and tiny holes in the slurry layer caused by thermal stress during direct drying, and enhance the bonding strength between the slurry layer and the workpiece surface.
[0050] S140, placing the workpiece with the pre-sprayed layer in an inert atmosphere for laser cladding treatment, and obtaining an aluminide cladding coating after cooling.
[0051] In some preferred embodiments, in the laser cladding process, the laser power is 2-2.8 KW, the scanning rate is 20-40 mm / s, the spot diameter is 2-5 mm, the workpiece rotation speed is 0-5 r / min, and the Ar gas flow rate is 15-20 L / min.
[0052] It should be understood that after the aluminide cladding coating is obtained, the residue on the surface of the workpiece should also be processed, for example, by flushing the residue on the surface of the workpiece with a high-pressure water gun or a high-pressure air flow, and then drying it naturally.
[0053] In other preferred embodiments, the thickness of the obtained aluminide cladding coating is 1.15-2.95 mm.
[0054] The method of this embodiment is suitable for preparing anti-oxidation coatings of austenitic steel and high-temperature alloy parts used for large boilers, oil and gas field transportation pipelines and other workpieces with large aspect ratios and various complex shapes.
[0055] In this embodiment, a thicker aluminide cladding coating can be obtained by combining the laser cladding process with aluminizing. The process has concentrated heat, short action time, small thermal impact in the cladding zone, high bonding strength between the coating and the base material, high coating production efficiency, controllable thickness, high process repeatability, and is extremely practical and universal.
[0056] In this embodiment, an aluminide cladding coating with a thickness of 1.15-2.95 mm and good metallurgical bonding with the substrate is prepared by adjusting main process parameters such as the content of solid phase cladding components, the content of modifier addition, the thickness of the spray layer and laser cladding parameters. The obtained aluminide cladding coating has an oxidation resistance that is 19-65 times higher than that of the parent material in a 600°C pure water vapor environment and 20-78 times higher than that of the parent material in a 650°C pure water vapor environment. This shows that the aluminide cladding coating prepared by this method effectively improves the oxidation resistance of the alloy parent material in a water vapor environment.
[0057] The following is a method for improving the corrosion resistance of the aluminide cladding coating in combination with several specific embodiments:
[0058] Example 1
[0059] Step 1. Weigh the solid phase components according to the mass ratio, including 50% NiAl, 40% Al, 2% NH4Cl, 4% Si and 4% Pt, place it in a planetary ball mill at 400 rpm for 12 hours to obtain a solid phase cladding powder; then, add 10% ethyl acetate and stir it for 4 hours, then place it in a planetary ball mill at 400 rpm for 12 hours, and after completion, a uniformly mixed slurry is obtained, which is the cladding slurry.
[0060] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 45 minutes, and use spraying to pre-set the slurry layer thickness to 3mm, keeping the coating coverage rate not less than 98%; then, air dry the workpiece naturally for 48 hours, and cure it at 450°C for 48 hours.
[0061] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2KW, the scanning rate is 40mm / s, the spot diameter is 5mm, the workpiece rotation speed is 5r / min, and the Ar gas flow rate is 20L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is flushed with high-pressure airflow to obtain an aluminide cladding coating with a thickness of 2.35mm, as shown in Table 1.
[0062] Example 2
[0063] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser power in the laser processing parameters of step 3 is changed to 2.8KW. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.45mm, as shown in Table 1.
[0064] Example 3
[0065] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser power in the laser processing parameters of step 3 is changed to 2.8KW, the scanning rate is 20mm / s, the Ar gas flow rate is 15L / min, and the rotation speed is 4r / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.18mm, as shown in Table 1.
[0066] Example 4
[0067] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser power in the laser processing parameters of step 3 is changed to 2.8KW, the scanning rate is 20mm / s, the spot diameter is 2mm, and the Ar gas flow rate is 15L / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 1.15mm, as shown in Table 1.
[0068] like Figure 2 As shown, according to the cross-sectional morphology, the diffusion layer has a uniform structure, moderate thickness, sufficient diffusion of Al atoms, and a good metallurgical bond between the diffusion layer and the matrix, which is not easy to fall off.
[0069] Example 5
[0070] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser processing parameters in step 3 are changed to laser power of 2.5KW, scanning rate of 30mm / s, spot diameter of 2mm, Ar gas flow rate of 18L / min, and rotation speed of 2r / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 1.54mm, as shown in Table 1.
[0071] Example 6
[0072] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser processing parameters in step 3 are changed to laser power of 2.4KW, scanning rate of 25mm / s, spot diameter of 2mm, Ar gas flow rate of 15L / min, and rotation speed of 2r / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.32mm, as shown in Table 1.
[0073] Example 7
[0074] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser power in the laser processing parameters of step 3 is changed to 2.8KW, the scanning rate is 35mm / s, and the spot diameter is 3mm. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.41mm, as shown in Table 1.
[0075] Example 8
[0076] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser processing parameters in step 3 are changed to laser power of 2.6KW, scanning rate of 25mm / s, spot diameter of 3mm, Ar gas flow rate of 18L / min, and rotation speed of 4r / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.37mm, as shown in Table 1.
[0077] Example 9
[0078] The steps of this example are the same as those of Example 1, and the same ratio of solid-phase cladding powder and liquid-phase binder is maintained. The difference is that the laser power in the laser processing parameters of step 3 is changed to 2.8KW, the spot diameter is 4mm, and the rotation speed is 4r / min. After treatment, the thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.68mm, as shown in Table 1.
[0079] In summary, according to Examples 1-9, the thickness of the diffusion layer is about 1.15-2.95 mm. More preferably, the thickness of the diffusion layer is greater than 2 mm, which is much higher than the current coating thickness and meets the long-term application requirements of the pipe.
[0080] Table 1 Laser cladding process parameters and coating thickness of Examples 1-9
[0081]
[0082]
[0083] Example 10
[0084] Step 1. Weigh the solid phase components according to the mass ratio, including 70% NiAl, 15% Al, 5% NH4Cl, 5% Si and 5% Pt, place it in a planetary ball mill at 350 rpm for 24 hours to obtain a solid phase cladding powder; then, add 30% ethyl acetate and stir it for 2 hours, then place it in a planetary ball mill at 400 rpm for 12 hours, and after completion, a uniformly mixed slurry is obtained, which is the cladding slurry.
[0085] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 200°C for 60 minutes, and use spraying to pre-set the slurry layer thickness to 5mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece for 24 hours and cure it at 300°C for 48 hours.
[0086] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2.5KW, the scanning rate is 20mm / s, the spot diameter is 2mm, the workpiece rotation speed is 5r / min, and the Ar gas flow rate is 15L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is flushed with high-pressure airflow. The thickness of the aluminide cladding coating formed on the surface of the workpiece is 1.65mm, as shown in Table 2.
[0087] Embodiment 11
[0088] Step 1. Weigh the solid phase components according to the mass ratio, including 50% NiAl, 40% Al, 5% NH4Cl and 5% Pt, place it in a planetary ball mill at 400 rpm for 24 hours to obtain a solid phase cladding powder; then, add 20% ethyl acetate and stir it for 2 hours, then place it in a planetary ball mill at 350 rpm for 8 hours, and after completion, obtain a uniformly mixed slurry, which is the cladding slurry.
[0089] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 30 minutes, and use spraying to pre-set the slurry layer thickness to 2mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece for 24 hours and cure it at 450°C for 48 hours.
[0090] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2.8KW, the scanning rate is 40mm / s, the spot diameter is 3mm, the workpiece rotation speed is 2r / min, and the Ar gas flow rate is 15L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is flushed with high-pressure airflow. The thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.36mm, as shown in Table 2.
[0091] Example 12
[0092] Step 1. Weigh the solid phase components according to the mass ratio, including 50% NiAl, 40% Al, 5% NH4Cl and 5% Si, place it in a planetary ball mill at 400 rpm for 12 hours to obtain a solid phase cladding powder; then, add 20% ethyl acetate and stir it for 2 hours, then place it in a planetary ball mill at 350 rpm for 12 hours, and after completion, obtain a uniformly mixed slurry, which is the cladding slurry.
[0093] Step 2: Clean the surface of the workpiece with a high-pressure water gun for 5 minutes and rinse it with alcohol or acetone; then, preheat the workpiece at 200°C for 60 minutes, and use spraying to pre-set the slurry layer thickness to 5mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece for 24 hours and cure it at 400°C for 48 hours.
[0094] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2.8KW, the scanning rate is 20mm / s, the spot diameter is 3mm, the workpiece rotation speed is 5r / min, and the Ar gas flow rate is 15L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is flushed with high-pressure airflow. The thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.43mm, as shown in Table 2.
[0095] Embodiment 13
[0096] Step 1. Weigh the solid phase components according to the mass ratio, including 60% NiAl, 30% Al, 5% Si and 5% Pt, place it in a planetary ball mill at 400 rpm for 24 hours to obtain a solid phase cladding powder; then, add 30% ethyl acetate and stir it for 2 hours, then place it in a planetary ball mill at 400 rpm for 12 hours, and after completion, obtain a uniformly mixed slurry, which is the cladding slurry.
[0097] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 45 minutes, and use spraying to pre-set the slurry layer thickness to 5mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece for 24 hours and cure it at 450°C for 48 hours.
[0098] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2KW, the scanning rate is 30mm / s, the spot diameter is 5mm, the workpiece rotation speed is 5r / min, and the Ar gas flow rate is 18L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is washed with high-pressure airflow. The thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.40mm, as shown in Table 2.
[0099] Embodiment 14
[0100] Step 1. Weigh the solid phase components according to the mass ratio, including 65% NiAl, 25% Al, 2% NH4Cl, 4% Si and 4% Pt, place it in a planetary ball mill at 350 rpm for 12 hours to obtain a solid phase cladding powder; then, add 30% ethyl acetate and stir it for 4 hours, then place it in a planetary ball mill at 400 rpm for 8 hours, and after completion, a uniformly mixed slurry is obtained, which is the cladding slurry.
[0101] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 60 minutes, and use spraying to pre-set the slurry layer thickness to 4mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece for 36 hours and cure it at 450°C for 48 hours.
[0102] Step 3: Place the workpiece under Ar for laser cladding, with a laser power of 2.8KW, a scanning rate of 40mm / s, a spot diameter of 5mm, a workpiece rotation speed of 4r / min, and an Ar gas flow rate of 20L / min; after completion, cool to room temperature and flush the residue on the workpiece surface with high-pressure airflow. The thickness of the aluminide cladding coating formed on the workpiece surface is 2.42mm, as shown in Table 2.
[0103] Embodiment 15
[0104] Step 1. Weigh the solid phase components according to the mass ratio, including 65% NiAl, 25% Al, 4% NH4Cl, 2% Si and 4% Pt, place it in a planetary ball mill at 350 rpm for 24 hours to obtain a solid phase cladding powder; then, add 20% ethyl acetate and stir it thoroughly for 4 hours, then place it in a planetary ball mill at 400 rpm for 8 hours, and after completion, a uniformly mixed slurry is obtained, which is the cladding slurry.
[0105] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 60 minutes, and use spraying to pre-set the slurry layer thickness to 5mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece naturally for 48 hours, and cure it at 450°C for 48 hours.
[0106] Step 3: Place the workpiece under Ar for laser cladding, with a laser power of 2.8KW, a scanning rate of 40mm / s, a spot diameter of 4mm, a workpiece rotation speed of 4r / min, and an Ar gas flow rate of 15L / min; after completion, cool to room temperature and flush the residue on the workpiece surface with high-pressure airflow. The thickness of the aluminide cladding coating formed on the workpiece surface is 2.73mm, as shown in Table 2.
[0107] Example 16
[0108] Step 1. Weigh the solid phase components according to the mass ratio, including 65% NiAl, 30% Al, 1% NH4Cl, 2% Si and 2% Pt, place it in a planetary ball mill at 400 rpm for 24 hours to obtain a solid phase cladding powder; then, add 30% ethyl acetate and stir it for 4 hours, then place it in a planetary ball mill at 400 rpm for 8 hours, and after completion, a uniformly mixed slurry is obtained, which is the cladding slurry.
[0109] Step 2: Use a high-pressure water gun to clean the surface of the workpiece for 5 minutes, and rinse it with alcohol or acetone; then, preheat the workpiece at 250°C for 60 minutes, and use spraying to pre-set the slurry layer thickness to 5mm, keeping the coating coverage rate not less than 98%; then, air-dry the workpiece naturally for 24 hours, and cure it at 450°C for 48 hours.
[0110] Step 3, the workpiece is placed under Ar for laser cladding, the laser power is 2.8KW, the scanning rate is 35mm / s, the spot diameter is 4mm, the workpiece rotation speed is 2r / min, and the Ar gas flow rate is 18L / min; after completion, it is cooled to room temperature and the residue on the surface of the workpiece is flushed with high-pressure airflow. The thickness of the aluminide cladding coating formed on the surface of the workpiece is 2.77mm, as shown in Table 2.
[0111] In summary, according to Examples 10-16, by changing the ratio of the solid-phase cladding powder, the thickness of the obtained penetration layer is mostly above 2 mm. This shows that when the components of the solid-phase cladding powder are within the above-mentioned ratio range and the laser cladding treatment process parameters are also within the range given above, the thickness of the obtained coating is mostly above 2 mm, which effectively improves the service life of the pipe.
[0112] Table 2 Laser cladding process parameters and coating thickness of Examples 10-16
[0113]
[0114] The present disclosure proposes a method for improving the corrosion resistance of an aluminide cladding coating, which has the following beneficial effects compared to the prior art:
[0115] First, the present disclosure adds halide NH4Cl to the slurry component, which has the effect of promoting penetration and activation, thereby improving the penetration rate and coating quality;
[0116] Second, the present invention introduces modified elements Si and Pt into the solid phase powder to accelerate the oxide film transformation process and form an insoluble silicon oxide protective layer, thereby enhancing the oxidation and corrosion resistance of the coating;
[0117] Third, the present invention prepares the coating by laser cladding process, which has concentrated heat, short action time, small thermal impact in the cladding area, and high bonding strength between the coating and the base material;
[0118] Fourth, the present invention prepares the coating through an integrated laser cladding process production line, the coating production efficiency is high, the thickness is controllable, the process repeatability is high, and it has strong practicality and universality;
[0119] Fifth, the method disclosed in the present invention is applicable to austenitic steel and high-temperature alloy components used in large boilers, oil and gas field transportation pipelines and other workpieces with large aspect ratios and various complex shapes. It has strong practicality, high permeation rate, excellent membrane-base bonding, and excellent industrial mass production benefits.
[0120] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.
Claims
1. A method for improving the corrosion resistance of an aluminide cladding coating, characterized in that: The method comprises: The solid phase cladding powder and the liquid phase binder are mixed, stirred and ball milled to obtain a cladding slurry; Clean and preheat the surface of the workpiece to be plated; Spraying the cladding slurry onto the surface of the workpiece to be plated, drying and curing the workpiece to form a pre-sprayed layer on the workpiece surface; The workpiece with the pre-sprayed layer is placed in an inert atmosphere for laser cladding treatment, and an aluminide cladding coating is obtained after cooling.
2. The method according to claim 1, characterized in that The solid phase cladding powder comprises an aluminum infiltration source, a modifier and an activator.
3. The method according to claim 2, characterized in that The aluminum diffusion sources are NiAl and Al.
4. The method according to claim 2, characterized in that: The modifiers are Si and Pt.
5. The method according to claim 2, characterized in that: The activating agent is NH4Cl.
6. The method according to any one of claims 2 to 5, characterized in that: The content of NiAl is 50-70%; The content of Al is 15-40%; The content of Si is 0-5%; The content of Pt is 0-5%; The content of NH4Cl is 0-5%.
7. The method according to claim 1, characterized in that The liquid phase binder is any one of ethyl acetate, polyvinyl alcohol, sodium carboxymethyl cellulose and nitrocellulose.
8. The method according to claim 7, characterized in that The content of the liquid phase binder is 10-30% of the mass of the solid phase cladding powder.
9. The method according to claim 1, characterized in that: In the laser cladding process, the laser power is 2-2.8KW, the scanning rate is 20-40mm / s, the spot diameter is 2-5mm, the workpiece rotation speed is 0-5r / min, and the Ar gas flow rate is 15-20L / min.
10. The method according to claim 1, characterized in that The thickness of the spray coating is 1-5 mm; The thickness of the aluminide cladding coating is 1.15-2.95 mm.
Citation Information
Patent Citations
Laser cladding method for preparing nickel-based heat-resisting and wear-resisting coating on surface of zirconium alloy
CN103866319A
High-entropy alloy material and preparation method of cladding layer
CN106244887A
High-temperature TiAl-based laser cladding alloy coating and preparation method thereof
CN107043873A
Method for preparing AlxCoCrNiMnTi high entropy alloy coating by using axial flow laser and coating prepared according to method
CN110331400A
Method for preparing TiC / TiB wear-resisting coating in in-situ manner through laser cladding
CN111005019A
Cited By
Rare earth element modification method for aluminide cladding coating
CN119824407A
Aluminum-based cladding coating and modification method thereof
CN119859784A
Modification method for improving corrosion resistance of aluminide anti-oxidation coating
CN120006279A
Modification method for improving corrosion resistance of chromium-nickel cladding coating
CN120006280A
Method for modifying aluminide coating based on laser cladding
CN120006281A