Rapidly formed photosensitive resin and application thereof
By optimizing the composition and molding process of photosensitive resin, the problems of low solid content and poor precision of alumina ceramics are solved, and efficient and low-cost ceramic molding is achieved, which is suitable for rapid molding of complex structures and hollow porous ceramic parts.
Patent Information
- Application Number
- CN202410802436.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
Existing alumina ceramics have low alumina solid content and poor accuracy, which makes the processing of ceramic parts difficult and costly.
A rapid prototyping photosensitive resin is used, including component A and component B. Component A is composed of polyurethane acrylate oligomer, bifunctional acrylate monomer and multifunctional acrylate monomer, adding photocuring agent and dispersion Agent, ceramic slurry is prepared through light curing technology to achieve high solid content and high precision 3D printing.
It achieves high solid content and high-precision molding of alumina ceramics, shortens the production cycle, reduces process costs, and at the same time improves the printing rate and the fluidity, flexibility and wear resistance of the product.
Smart Images

Figure CN118732391A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of 3D printing ceramic materials, and in particular to a photosensitive resin for rapid prototyping and its application Background Art
[0002] Ceramics are widely used in chemical industry, machinery, electronics, aerospace, biomedicine and other fields due to their excellent mechanical strength, high temperature resistance, chemical stability, and physical properties such as acoustics, light, electromagnetics and heat. As a product of the combination of traditional materials and modern new technologies, its advantages also make it more and more widely used in various fields. Traditional ceramic manufacturing processes generally require pre-manufacturing of molds, resulting in a long overall production cycle and the inability to form ceramic parts with highly complex structures, especially hollow and porous ones. Ceramics are extremely hard and brittle, and are difficult to process, so it is difficult to process them into complex structures and shapes to meet various application requirements. With the rapid development of 3D printing technology, its application in the field of ceramic parts manufacturing also provides new possibilities for solving the above problems and challenges.
[0003] 3D printing of ceramics was proposed by American scholars as early as the 1990s. With the rapid development of the computer and material fields, 3D printing technology suitable for ceramics has been constantly updated, with wider application coverage and better performance. Among them, digital light curing technology (DLP technology) has become a hot topic of research because of its low printing cost and ability to achieve fast, high-precision, and high-complexity printing from surface to body. DLP uses UV light to solidify the photocurable medium to obtain a green body, but unlike SLA, which uses UV lasers to complete a layer of printing from point to line and line to surface, DLP uses a UV projector to directly complete the curing of a layer, making it faster than the traditional SLA point and line layer scanning process, and the time used for 3D printing is also shortened.
[0004] Alumina ceramics have excellent properties such as good heat resistance, high mechanical strength, good thermal conductivity, low thermal expansion coefficient, and corrosion resistance. They are widely used in biomedicine, batteries and other fields. Using DLP technology to achieve fast and high-precision printing of complex structures of alumina ceramics is also one of the current research hotspots. However, the process cost of DLP technology printing alumina is high and it is difficult to achieve high solid content. Therefore, photosensitive resins that can cure quickly and achieve high solid content are urgently needed. Summary of the invention
[0005] Based on this, in order to solve the problems of low alumina solid content and poor precision of existing alumina ceramics, the present invention provides a rapid prototyping photosensitive resin and its application, and the specific technical solution is as follows:
[0006] A rapid prototyping photosensitive resin, the photosensitive resin comprising component A and component B, the component A comprising the following components in percentage by mass: 35% to 40% of polyurethane acrylate oligomer, 35% to 40% of bifunctional acrylate monomer, and 20% to 30% of multifunctional acrylate monomer; the component B comprising 0.5% to 2% of the mass of the component A in terms of a photocuring agent and 0.5% to 2% of the mass of the component A in terms of a dispersant.
[0007] Furthermore, the polyurethane acrylate oligomer is an aliphatic polyurethane acrylate with a functionality of 2 to 6.
[0008] Furthermore, the bifunctional acrylate monomer is tripropylene glycol diacrylate.
[0009] Furthermore, the multifunctional acrylate monomer is ethoxylated pentaerythritol tetraacrylate.
[0010] Furthermore, the photocuring agent is 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide.
[0011] Furthermore, the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:(1-3).
[0012] In addition, the present invention provides an application of a photosensitive resin, wherein the application is an application of the photosensitive resin in the preparation of photocurable ceramics.
[0013] Furthermore, the preparation of the light-cured ceramic comprises the following steps:
[0014] Adding polyurethane acrylate oligomer, bifunctional acrylate monomer and multifunctional acrylate monomer into a homogenizer, and then adding a photocuring agent and a dispersant, stirring at a speed of 200 r / min for 1 h to 2 h under the action of magnetic stirring, and then placing in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 min to fully dissolve the photocuring agent and fully mix the components to obtain a photosensitive resin;
[0015] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, and the speed of each homogenization is 300r / min to 800r / min, and the homogenization time is 5min to 20min, to obtain a ceramic slurry;
[0016] Setting light-curing parameters, importing the design model, and performing light-curing 3D printing on the ceramic slurry to obtain a green body;
[0017] The surface of the green body is cleaned, dried, and subjected to binder removal and sintering treatments to obtain a ceramic product.
[0018] Further, the debinding treatment is as follows: heating from room temperature to 180°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; then heating from 180°C to 240°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; then heating from 240°C to 400°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; then heating from 400°C to 460°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; then heating from 460°C to 600°C at a heating rate of 0.5°C / min to 1°C / min, and keeping warm for 120min to 180min, and then cooling to room temperature.
[0019] Furthermore, the sintering treatment is: heating from room temperature to 1000°C at a heating rate of 8°C / min to 10°C / min, then heating to 1550°C at a heating rate of 3°C / min to 5°C / min, and keeping the temperature for 2h to 4h.
[0020] In the above scheme, a polyurethane acrylate oligomer with low viscosity, high activity and good yellowing resistance, a bifunctional acrylate monomer with excellent shear force, and a multifunctional acrylate monomer with high hardness, good wear resistance and high reaction activity are compounded, so that the cross-linking density of the photosensitive resin after curing can be improved, so that the photosensitive resin can be quickly formed, and the prepared photosensitive resin has excellent fluidity, flexibility, wear resistance and service life; the prepared photosensitive resin is applied to ceramic slurry to prepare various ceramic products, which can achieve a high solid content of aluminum oxide in the ceramic products, fast molding speed, high precision, save costs and improve printing rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the rheological properties of the photosensitive resin in Example 1 of the present invention;
[0022] Figure 2 Schematic diagram of rheological properties of 80% ceramic slurry prepared in Example 1 of the present invention;
[0023] Figure 3 Schematic diagram of comparison of printed samples in Application Example 1 of the present invention, wherein: Figure 3 a in the figure is a three-dimensional model. Figure 3 b in the figure is the printed blank;
[0024] Figure 4 This is a schematic diagram of a thermogravimetric analysis curve of an 80% ceramic slurry prepared in Example 1 of the present invention;
[0025] Figure 5It is a schematic diagram of the binder removal sintering curve of the 80% ceramic slurry prepared in Example 1 of the present invention;
[0026] Figure 6 Schematic diagram showing the comparison of curing depths at different photocuring agent addition amounts in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0029] A photosensitive resin for rapid prototyping in one embodiment of the present invention comprises component A and component B, wherein component A comprises the following ingredients in percentage by mass: 35% to 40% of polyurethane acrylate oligomer, 35% to 40% of bifunctional acrylate monomer, and 20% to 30% of multifunctional acrylate monomer; and component B comprises 0.5% to 2% of a photocuring agent accounting for 0.5% to 2% of the mass of component A and 0.5% to 2% of a dispersant accounting for 0.5% to 2% of the mass of component A.
[0030] In one embodiment, the polyurethane acrylate oligomer is an aliphatic polyurethane acrylate with a functionality of 2 to 6.
[0031] In one embodiment, the bifunctional acrylate monomer is tripropylene glycol diacrylate.
[0032] In one embodiment, the multifunctional acrylate monomer is ethoxylated pentaerythritol tetraacrylate.
[0033] In one embodiment, the photocuring agent is 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide.
[0034] In one embodiment, the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:(1-3).
[0035] In addition, the present invention provides an application of a photosensitive resin, wherein the application is an application of the photosensitive resin in the preparation of photocurable ceramics.
[0036] In one embodiment, the preparation of the light-cured ceramic comprises the following steps:
[0037] Adding polyurethane acrylate oligomer, bifunctional acrylate monomer and multifunctional acrylate monomer into a homogenizer, and then adding a photocuring agent and a dispersant, stirring at a speed of 200 r / min for 1 h to 2 h under the action of magnetic stirring, and then placing in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 min to fully dissolve the photocuring agent and fully mix the components to obtain a photosensitive resin;
[0038] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, and the speed of each homogenization is 300r / min to 800r / min, and the homogenization time is 5min to 20min, to obtain a ceramic slurry;
[0039] Setting light-curing parameters, importing the design model, and performing light-curing 3D printing on the ceramic slurry to obtain a green body;
[0040] The surface of the green body is cleaned, dried, and subjected to binder removal and sintering treatments to obtain a ceramic product.
[0041] In one embodiment, the debinding treatment is as follows: heating from room temperature to 180°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; heating from 180°C to 240°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; heating from 240°C to 400°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; heating from 400°C to 460°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 30min to 60min; heating from 460°C to 600°C at a heating rate of 0.5°C / min to 1°C / min, and keeping warm for 120min to 180min, and then cooling to room temperature.
[0042] In one embodiment, the sintering treatment is: heating from room temperature to 1000°C at a heating rate of 8°C / min to 10°C / min, then heating to 1550°C at a heating rate of 3°C / min to 5°C / min, and keeping the temperature for 2h to 4h.
[0043] In one embodiment, the average particle size of the alumina powder is 1 μm to 10 μm.
[0044] In one of the embodiments, in the ceramic slurry, the mass fraction of alumina powder is 60% to 80%.
[0045] In one embodiment, the alumina powder is treated at a temperature of 70° C. to 100° C. for 10 min to 3 h before use.
[0046] By optimizing the ingredients for compounding in the above scheme, the cross-linking density of the photosensitive resin after curing can be increased, so that the photosensitive resin can be quickly molded, and the prepared photosensitive resin has excellent fluidity, flexibility, wear resistance and service life; the prepared photosensitive resin is applied to ceramic slurry to prepare various ceramic products, which can achieve a high solid content of alumina in the ceramic products, fast molding speed, high precision, saving costs while also improving the printing rate.
[0047] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0048] Embodiment 1:
[0049] The alumina powder was placed at 100°C for 30 minutes;
[0050] According to the composition by mass percentage, 38% polyurethane acrylate, 37% tripropylene glycol diacrylate and 25% ethoxylated pentaerythritol tetraacrylate are stirred and defoamed in a homogenizer to obtain component A, and then 0.5% of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide by mass of the component A is added, and 1% of a dispersant by mass of the component A is added, and the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:1, and stirred at a speed of 200 r / min for 1 hour, and then placed in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 minutes, so that the photocuring agent is fully dissolved and the components are fully mixed to obtain a photosensitive resin;
[0051] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, with the speed of each homogenization being 300 r / min and the homogenization time being 10 min, to obtain a ceramic slurry with an alumina mass fraction of 80%.
[0052] Figure 1 As shown, the viscosity of the photosensitive resin in Example 1 is 150 mpa·s, which has excellent fluidity. The viscosity of the ceramic slurry obtained in Example 1 is 800 mpa·s. Figure 2 The overall viscosity is low, the fluidity is excellent, the stability is good, and no sedimentation occurs after standing for 3 days, which makes it suitable for 3D printing.
[0053] Embodiment 2:
[0054] The alumina powder was placed at 80°C for 30 minutes;
[0055] According to the composition by mass percentage, 35% of polyurethane acrylate, 40% of tripropylene glycol diacrylate and 25% of ethoxylated pentaerythritol tetraacrylate are stirred and defoamed in a homogenizer to obtain component A, and then 0.5% of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide by mass of the component A is added, and 1% of a dispersant by mass of the component A is added, and the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:3, and stirred at a speed of 200 r / min for 1 hour, and then placed in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 minutes, so that the photocuring agent is fully dissolved and the components are fully mixed to obtain a photosensitive resin;
[0056] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, with the speed of each homogenization being 300 r / min and the homogenization time being 10 min, to obtain a ceramic slurry with an alumina mass fraction of 80%.
[0057] The photosensitive resin and ceramic slurry obtained in Example 2 both have excellent fluidity. The ceramic slurry has a viscosity of 700 mPa·s and good stability. No sedimentation occurs after standing for 3 days, and is suitable for 3D printing.
[0058] Embodiment 3:
[0059] The alumina powder was placed at 95°C for 30 minutes;
[0060] According to the composition by mass percentage, 40% of polyurethane acrylate, 35% of tripropylene glycol diacrylate and 25% of ethoxylated pentaerythritol tetraacrylate are stirred and defoamed in a homogenizer to obtain component A, and then 0.5% of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide by mass of the component A is added, and 1% of a dispersant by mass of the component A is added, and the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:3, and stirred at a speed of 200 r / min for 1 hour, and then placed in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 minutes, so that the photocuring agent is fully dissolved and the components are fully mixed to obtain a photosensitive resin;
[0061] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, with the speed of each homogenization being 300 r / min and the homogenization time being 10 min, to obtain a ceramic slurry with an alumina mass fraction of 80%.
[0062] The photosensitive resin and ceramic slurry obtained in Example 3 both have excellent fluidity. The ceramic slurry has a viscosity of 1200 mpa·s and good stability. No sedimentation occurs after standing for 3 days, and is suitable for 3D printing.
[0063] Application Example 1:
[0064] Set the light curing parameters, import the design model, and perform light curing 3D printing on the ceramic slurry prepared in Example 1 to obtain a green body. Clean the surface of the green body, dry it, and heat it from room temperature to 180°C at a heating rate of 1°C / min, and keep it warm for 45 minutes; then heat it from 180°C to 240°C at a heating rate of 2°C / min, and keep it warm for 45 minutes; then heat it from 240°C to 400°C at a heating rate of 1°C / min, and keep it warm for 60 minutes; then heat it from 400°C to 460°C at a heating rate of 2°C / min, and keep it warm for 30 minutes; then heat it from 460°C to 600°C at a heating rate of 1°C / min, and keep it warm for 120 minutes, then cool it down to room temperature to complete the debinding. Then heat it from room temperature to 1000°C at a heating rate of 8°C / min, and then heat it to 1550°C at a rate of 5°C / min, and keep it warm for 2 hours to obtain a finished ceramic product.
[0065] like Figure 3 As shown, Figure 3 a in the figure is a three-dimensional model. The exposure time is adjusted to 1000ms, the curing depth is set to 200 microns, and the layer thickness is set to 50 microns. The green body with a three-dimensional porous structure is obtained, as shown in FIG. Figure 3 As shown in b, the surface of the green body is smooth.
[0066] Comparative Example 1:
[0067] The difference between Comparative Example 1 and Example 1 is that the amount of the photocuring agent added in Comparative Example 1 is different. The amount of the photocuring agent added in Comparative Example 1 accounts for 3% by weight of the component A. The rest is the same as Example 1.
[0068] In Comparative Example 1, a ceramic slurry with a mass fraction of 80% was prepared. Due to the different amount of curing agent added, the curing depth in Comparative Example 1 was better than that in Example 1. Due to the increase in the photocuring agent, more short-chain polymerization reactions were initiated, but due to excessive reaction, the cured edge was overexposed and caused "serrated" phenomenon, which made the printed body rough.
[0069] Comparative Example 2:
[0070] The alumina powder was placed at 100°C for 30 minutes;
[0071] According to the composition by mass percentage, 45% of polyurethane acrylate, 45% of tripropylene glycol diacrylate and 10% of ethoxylated pentaerythritol tetraacrylate are stirred and defoamed in a homogenizer to obtain component A, and then 0.5% of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide by mass of the component A is added, and 1% of a dispersant by mass of the component A is added, and the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:1, and stirred at a speed of 200 r / min for 1 hour, and then placed in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 minutes, so that the photocuring agent is fully dissolved and the components are fully mixed to obtain a photosensitive resin;
[0072] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, with the speed of each homogenization being 300 r / min and the homogenization time being 10 min, to obtain a ceramic slurry with an alumina mass fraction of 80%.
[0073] The viscosity of the ceramic slurry obtained in Comparative Example 2 is 6500 mPa·s, which is relatively high and easily causes slurry accumulation during printing, which is not conducive to 3D printing.
[0074] Comparative Example 3:
[0075] The alumina powder was placed at 100°C for 30 minutes;
[0076] According to the composition by mass percentage, 30% of polyurethane acrylate, 40% of tripropylene glycol diacrylate and 30% of ethoxylated pentaerythritol tetraacrylate are stirred and defoamed in a homogenizer to obtain component A, and then 0.5% of 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide by mass of the component A is added, and 1% of a dispersant by mass of the component A is added, and the dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:1, and stirred at a speed of 200 r / min for 1 hour, and then placed in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 minutes, so that the photocuring agent is fully dissolved and the components are fully mixed to obtain a photosensitive resin;
[0077] The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, with the speed of each homogenization being 300 r / min and the homogenization time being 10 min, to obtain a ceramic slurry with an alumina mass fraction of 80%.
[0078] The viscosity of the ceramic slurry obtained in Comparative Example 3 was 2500 mpa·s, which was relatively low. It settled after standing for 1 day, which was not conducive to 3D printing.
[0079] In summary, the present application can obtain a ceramic slurry with excellent viscosity and stability by optimizing the composition and ratio of the photosensitive resin, which is suitable for 3D printing.
[0080] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0081] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A photosensitive resin for rapid prototyping, characterized in that: The photosensitive resin includes component A and component B, wherein component A includes the following ingredients in percentage by mass: 35% to 40% of polyurethane acrylate oligomer, 35% to 40% of bifunctional acrylate monomer, and 20% to 30% of multifunctional acrylate monomer; and component B includes 0.5% to 2% of the mass of component A in terms of a photocuring agent and 0.5% to 2% of the mass of component A in terms of a dispersant.
2. The photosensitive resin according to claim 1, characterized in that: The polyurethane acrylate oligomer is an aliphatic polyurethane acrylate with a functionality of 2 to 6.
3. The photosensitive resin according to claim 1, characterized in that: The bifunctional acrylate monomer is tripropylene glycol diacrylate.
4. The photosensitive resin according to claim 1, characterized in that: The multifunctional acrylate monomer is ethoxylated pentaerythritol tetraacrylate.
5. The photosensitive resin according to claim 1, characterized in that: The photocuring agent is 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide.
6. The photosensitive resin according to claim 1, characterized in that: The dispersant is composed of BYK-163 and BYK-111 in a mass ratio of 2:(1-3).
7. An application of a photosensitive resin, characterized in that: The photosensitive resin is the photosensitive resin according to any one of claims 1 to 6, and the application is the application of the photosensitive resin in the preparation of photocurable ceramics.
8. The use according to claim 7, characterized in that: The preparation of the light-cured ceramic comprises the following steps: Adding polyurethane acrylate oligomer, bifunctional acrylate monomer and multifunctional acrylate monomer into a homogenizer, and then adding a photocuring agent and a dispersant, stirring at a speed of 200 r / min for 1 h to 2 h under the action of magnetic stirring, and then placing in a homogenizer at a speed of 500 r / min for homogenization and defoaming for 3 min to fully dissolve the photocuring agent and fully mix the components to obtain a photosensitive resin; The photosensitive resin and alumina powder are mixed in proportion, and placed in a homogenizer for homogenization and defoaming for several times, and the speed of each homogenization is 300r / min to 800r / min, and the homogenization time is 5min to 20min, to obtain a ceramic slurry; Setting light-curing parameters, importing the design model, and performing light-curing 3D printing on the ceramic slurry to obtain a green body; The surface of the green body is cleaned, dried, and subjected to binder removal and sintering treatments to obtain a ceramic product.
9. The use according to claim 8, characterized in that: The debinding treatment is as follows: heating from room temperature to 180°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 30min to 60min; then heating from 180°C to 240°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 30min to 60min; then heating from 240°C to 400°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 30min to 60min; then heating from 400°C to 460°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 30min to 60min; then heating from 460°C to 600°C at a heating rate of 0.5°C / min to 1°C / min, and keeping the temperature for 120min to 180min, and then cooling to room temperature.
10. The use according to claim 8, characterized in that: The sintering treatment is as follows: heating from room temperature to 1000° C. at a heating rate of 8° C. / min to 10° C. / min, then heating to 1550° C. at a heating rate of 3° C. / min to 5° C. / min, and keeping the temperature for 2h to 4h.
Citation Information
Cited By
Resin composition and method for producing sheet using the resin composition
JP2025152912A
Resin composition and method for producing a sheet using the resin composition
JP7739510B1