High-flux anti-pollution composite nanofiltration membrane and preparation method thereof
By using highly chemically reactive functional groups and cationic polyamine monomers to perform interfacial polymerization in the nanofiltration membrane, a selective separation layer with high permeability and barrier properties is formed, which solves the problem of existing nanofiltration membranes in removing heavy metals and small molecule organic matter. It achieves the effects of high throughput and high desalination rate, extends the service life and improves stability.
Patent Information
- Application Number
- CN202411070788.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-15
AI Technical Summary
The nanofiltration membranes of existing household water purifiers are not effective in removing heavy metal ions, small molecular organic matter and some viruses, and reverse osmosis technology consumes high energy and has a large proportion of wastewater, and conventional nanofiltration membranes have low desalination rates under low pressure conditions. , short service life.
Polyamine monomers, cationic polyamine monomers and surfactants with highly chemically reactive functional groups are polymerized at the interface with acid chloride monomers in aqueous solutions to form a selective separation layer with high permeability and barrier properties. Preparation of high-flux anti-pollution composite nanofiltration membrane by regulating reaction conditions.
It achieves a high-flux nanofiltration membrane that operates stably at low pressure, improves the salt rejection rate and membrane flux, extends the service life, and enhances the removal ability of harmful substances.
Smart Images

Figure CN118767705A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of domestic water treatment, and in particular to a high-throughput anti-pollution composite nanofiltration membrane and a preparation method thereof. Background Art
[0002] At present, the household water purifiers on the market are mainly based on ultrafiltration, nanofiltration, and reverse osmosis technologies. Ultrafiltration technology mainly removes bacteria, viruses, colloids, silt, rust, etc., but cannot effectively remove harmful substances such as heavy metal ions, small molecular organic matter, and some viruses. Reverse osmosis technology can remove almost all substances other than water and produce ultrapure water, but it cannot retain trace elements that are beneficial to the human body. Because of its large osmotic pressure, it consumes a lot of energy to provide driving force, and its wastewater generation ratio is high, so it has many limitations in daily use. Conventional reverse osmosis membranes have a significantly reduced desalination rate under low pressure conditions, and cannot operate stably relying solely on tap water pressure.
[0003] The nanofiltration membranes prepared by the traditional IP method in the commercial market mainly rely on several single water-phase monomers such as m-phenylenediamine, piperazine (PIP), ethylenetriamine, polyethyleneimine, polyhexamethyleneguanidine hydrochloride, bisphenol A, and tetrahydronaphthylamine, but this practice limits the types and possibilities of nanofiltration membranes to a certain extent. For example, the nanofiltration membrane prepared with m-phenylenediamine as the single water-phase monomer can achieve a desalination rate of more than 90% for divalent salt ions, but due to its slow diffusion rate to the organic phase during interfacial polymerization, a "ridge-valley" shaped polyamide separation layer is formed with large roughness. Therefore, after a period of use, some soluble organic matter in the water will be intercepted by the "ridge-valley", causing membrane pollution and seriously affecting the service life of the membrane. For another example, the nanofiltration membrane prepared with piperazine as the water-phase monomer, although the reaction speed has been improved, is not very ideal for the retention of calcium ions in actual application, which greatly limits its application in water hardness removal. Summary of the invention
[0004] The present invention provides a high-throughput anti-pollution composite nanofiltration membrane and a preparation method thereof. The technical solution of the present invention is achieved as follows:
[0005] A method for preparing a high-throughput anti-pollution composite nanofiltration membrane comprises the following steps:
[0006] (1) adding an aqueous phase monomer having a highly chemically reactive functional group, a cationic aqueous phase monomer, and a surfactant to deionized water in sequence and dispersing them uniformly to prepare an aqueous phase solution;
[0007] (2) dissolving the acyl chloride monomer in an organic solvent to prepare an organic phase solution;
[0008] (3) cutting the porous ultrafiltration base membrane into a certain size, placing it in a membrane-making tool, and then pouring the prepared aqueous solution into it, dipping the porous ultrafiltration base membrane for a period of time, then pouring out the remaining liquid, and using an air knife to blow away the droplets on the membrane surface to obtain a membrane sheet;
[0009] (4) placing the membrane into another membrane-making tool, and then pouring the organic phase solution into it for interfacial polymerization;
[0010] (5) The membrane sheet after interfacial polymerization is taken out, placed in an oven for heat treatment, and finally immersed and rinsed in deionized water to obtain a high-throughput anti-pollution composite nanofiltration membrane.
[0011] Preferably, in step (1), the aqueous solution comprises: 0-2.0 wt% of highly chemically reactive polyamine monomers, 0.01-0.3 wt% of cationic polyamine monomers, 0.01-2.0 wt% of surfactants, and the remainder is deionized water.
[0012] Preferably, the polyamine monomer having a highly chemically reactive functional group is one or more of piperazine, 2,2'-dimethylpiperazine, 2,5-dimethylpiperazine, p-phenylenediamine, o-phenylenediamine, and mesitylenetriamine; the cationic polyamine monomer is one or more of diethylenetriamine, ethylenediamine, triethylenetetramine, and polyethylenepolyamine; and the reactive surfactant is one or more of camphorsulfonic acid, sodium camphorsulfonate, sodium phosphate, and disodium hydrogen phosphate.
[0013] Of course, it should be understood that the cationic polyamine monomers include but are not limited to the types listed above, and other cationic polyamine small molecules are also within the protection scope of the present invention.
[0014] Preferably, in step (2), in the organic phase solution, the monomer concentration of the acyl chloride monomer is 0.01-2.0wt%; the acyl chloride monomer is one or more of trimesoyl chloride, isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, glutaryl chloride, and fumaroyl chloride; and the organic solvent is one or more of n-hexane, cyclohexane, n-heptane, ISOPAR G, and ISOPAR L.
[0015] Of course, it should be understood that the acyl chloride monomers include but are not limited to the types listed, and other monomers within the scope of acyl chloride monomers are also within the protection scope of the present invention.
[0016] Preferably, in step (3), the porous ultrafiltration base membrane is a commercially available porous ultrafiltration membrane, which is any one of polysulfone, polyethersulfone, sulfonated polyethersulfone, polyacrylonitrile, polyvinylidene fluoride, and cellulose acetate; the average pore size of the porous ultrafiltration membrane is 0.03-0.1 μm, preferably 0.03-0.06 μm.
[0017] Preferably, in step (3), the porous ultrafiltration base membrane is prepared by the following method:
[0018] The polymer resin is added into N,N-dimethylacetamide or N,N-dimethylformamide to dissolve, and a porogen is added, and the mixture is stirred and dissolved at 60-90°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable casting solution;
[0019] After vacuum degassing, the prepared casting solution is coated on a non-woven fabric substrate, and the coated non-woven fabric substrate is immersed in a coagulation bath at 30-70° C. for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0020] Preferably, in the casting solution, the polymer resin accounts for 16-20wt%, the porogen accounts for 1-12wt%, and the balance is N,N-dimethylacetamide or N,N-dimethylformamide as a solvent; the polymer resin is any one or more of polysulfone, polyethersulfone, polyacrylonitrile, polyvinylidene fluoride, and cellulose acetate; the porogen is one or more of polyethylene glycol, propanol, isopropanol, glycerol, polyvinyl pyrrolidone, and polyethylene oxide; wherein the molecular weight of polyethylene glycol is 400-8000, polyvinyl pyrrolidone includes K30, K60, K70, K80, and K90, and the molecular weight of polyethylene oxide is 40000-1200000.
[0021] Preferably, in step (3), the time for dipping the porous ultrafiltration base membrane in the aqueous solution is 0.5-30 min, preferably 1-15 min.
[0022] Preferably, in step (4), the interfacial polymerization time is 0.5-20 min, preferably 0.5-5 min;
[0023] In step (5), the heat treatment temperature is 40-80°C, preferably 50-70°C; the heat treatment time is 0.5-30 min, preferably 1-10 min.
[0024] The embodiment of the present invention further provides a high-throughput anti-pollution composite nanofiltration membrane, which is prepared by the above-mentioned preparation method.
[0025] In summary, this embodiment has at least the following advantages:
[0026] 1. The present invention uses a new type of mixed water phase system, utilizes the characteristics of different monomers, and synergistically regulates the interfacial polymerization reaction process to form a selective separation layer with certain high permeability and barrier properties, and has a better desalination rate and membrane flux. The new type of mixed water phase system is composed of polyamine monomers with highly chemically reactive functional groups, cationic polyamine monomers with a fast diffusion rate in water, surfactants, etc. Through this new type of mixed water phase system and the acyl chloride oil phase system, interfacial polymerization reaction is carried out, and during the reaction process, the concentration of cationic polyamine monomers, interfacial polymerization reaction time, and post-treatment temperature and other influencing factors are regulated to achieve the preparation of a composite nanofiltration membrane with high flux and high desalination rate.
[0027] 2. The present invention regulates the surface roughness of the nanofiltration membrane by utilizing the difference in diffusion rates between amine monomers with highly chemically reactive functional groups and cationic polyamine monomers in the organic phase, thereby making the surface of the nanofiltration membrane smoother, thereby preparing a new type of high-throughput, anti-pollution composite nanofiltration membrane that can operate stably under low pressure.
[0028] In summary, the preparation method of the present invention is simple, operable and highly applicable. It can effectively regulate the performance of the high-throughput anti-pollution composite membrane according to the regulation of the components of the aqueous phase system and the control of the process, and has good commercial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0030] Figure 1 It is a structural schematic diagram of the film-making tooling;
[0031] Figure 2 Schematic diagram for comparing the water contact angles of Example 1 and the comparative example. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for preparing a high-throughput anti-pollution composite nanofiltration membrane, the preparation steps are as follows:
[0035] (1) 16 wt% of polymer resin is added to N,N-dimethylacetamide (DMAc) to dissolve, and 5 wt% of porogen is added, and the mixture is stirred and dissolved at 60°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable polymer resin casting solution. The prepared casting solution is then vacuum degassed and coated on a non-woven fabric substrate, which is then immersed in a coagulation bath for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0036] (2) Preparation of an aqueous phase solution: 0.5 wt % of piperazine, 0.05 wt % of diethylenetriamine with a molecular weight of 103.17, and 0.1 wt % of sodium camphorsulfonate were added to deionized water in sequence and dispersed evenly to prepare an aqueous phase solution.
[0037] Among them, the molecular structure of diethylenetriamine is as follows:
[0038]
[0039] The amino group of diethylenetriamine can react with the acyl chloride group in the organic phase solution. The reaction rate is fast and a dense polyamide active layer is easily formed. The unreacted amino group will provide a certain cation removal effect.
[0040] (3) Preparation of organic phase solution: Dissolve 0.1 wt % of trimesoyl chloride in an organic solvent, ISOPAR G, to prepare an organic phase solution.
[0041] (4) Cut the porous ultrafiltration membrane into a certain size and place it in Figure 1 In the membrane-making tool shown, excess water on the membrane surface is dried, and then the aqueous solution prepared in step (2) is poured into the ultrafiltration base membrane for 2 minutes.
[0042] (5) The membrane sheet treated in step (4) is then transferred to another membrane-making tool, and the organic phase solution prepared in step (3) is poured into it for interfacial polymerization. The dipping time is 2 minutes.
[0043] (6) The membrane sheet treated in step (5) is taken out, placed in an oven for heat treatment at 70° C. for 2 min, and finally immersed and rinsed in deionized water to obtain the high-flux anti-pollution composite membrane.
[0044] Example 2
[0045] A method for preparing a high-flux low-pressure composite membrane, the preparation steps are as follows:
[0046] (1) 16 wt% of polymer resin is added to N,N-dimethylacetamide (DMAc) to dissolve, and 5 wt% of porogen is added, and the mixture is stirred and dissolved at 60°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable polymer resin casting solution. The prepared casting solution is then vacuum degassed and coated on a non-woven fabric substrate, which is then immersed in a coagulation bath for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0047] (2) Preparation of an aqueous phase solution: 0.5 wt % of piperazine, 0.1 wt % of diethylenetriamine with a molecular weight of 103.17, and 0.1 wt % of sodium camphorsulfonate were added to deionized water in sequence and dispersed evenly to prepare an aqueous phase solution.
[0048] (3) Preparation of organic phase solution: Dissolve 0.1 wt % of trimesoyl chloride in an organic solvent, ISOPAR G, to prepare an organic phase solution.
[0049] (4) Cut the homemade porous ultrafiltration base membrane into a certain size and place it in a homemade membrane-making tool to dry excess water on the membrane surface, then pour the aqueous solution prepared in step (2) into the ultrafiltration base membrane for 2 minutes.
[0050] (5) The membrane sheet treated in step (4) is then transferred to another membrane-making tool, and the organic phase solution prepared in step (3) is poured into it for interfacial polymerization. The dipping time is 2 minutes.
[0051] (6) The membrane sheet treated in step (5) is taken out, placed in an oven for heat treatment at 70° C. for 2 min, and finally immersed and rinsed in deionized water to obtain the high-flux anti-pollution composite membrane.
[0052] Example 3
[0053] A method for preparing a high-flux low-pressure composite membrane, the preparation steps are as follows:
[0054] (1) 16 wt% of polymer resin is added to N,N-dimethylacetamide (DMAc) to dissolve, and 5 wt% of porogen is added, and the mixture is stirred and dissolved at 60°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable polymer resin casting solution. The prepared casting solution is then vacuum degassed and coated on a non-woven fabric substrate, which is then immersed in a coagulation bath for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0055] (2) Preparation of an aqueous phase solution: 0.3 wt % of piperazine, 0.05 wt % of diethylenetriamine with a molecular weight of 103.17, and 0.1 wt % of sodium camphorsulfonate were added to deionized water in sequence and dispersed evenly to prepare an aqueous phase solution.
[0056] (3) Preparation of organic phase solution: Dissolve 0.3 wt % of trimesoyl chloride in an organic solvent, ISOPAR G, to prepare an organic phase solution.
[0057] (4) Cut the homemade ultrafiltration base membrane into a certain size and place it in a homemade membrane-making tool to dry excess water on the membrane surface, then pour the aqueous solution prepared in step (2) into the ultrafiltration base membrane for 2 minutes.
[0058] (5) The membrane sheet treated in step (4) is then transferred to another membrane-making tool, and the organic phase solution prepared in step (3) is poured into it for interfacial polymerization. The dipping time is 2 minutes.
[0059] (6) The membrane sheet treated in step (5) is taken out, placed in an oven for heat treatment at 70° C. for 2 min, and finally immersed and rinsed in deionized water to obtain the high-flux anti-pollution composite membrane.
[0060] Example 4
[0061] A method for preparing a high-flux low-pressure composite membrane, the preparation steps are as follows:
[0062] (1) 16 wt% of polymer resin is added to N,N-dimethylacetamide (DMAc) to dissolve, and 5 wt% of porogen is added, and the mixture is stirred and dissolved at 60°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable polymer resin casting solution. The prepared casting solution is then vacuum degassed and coated on a non-woven fabric substrate, which is then immersed in a coagulation bath for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0063] (2) Preparation of an aqueous phase solution: 0.3 wt % of piperazine, 0.1 wt % of diethylenetriamine with a molecular weight of 103.17, and 0.1 wt % of sodium camphorsulfonate were added to deionized water in sequence and dispersed evenly to prepare an aqueous phase solution.
[0064] (3) Preparation of organic phase solution: Dissolve 0.1 wt % of trimesoyl chloride in an organic solvent, ISOPAR G, to prepare an organic phase solution.
[0065] (4) Cut the homemade ultrafiltration base membrane into a certain size and place it in a homemade membrane-making tool to dry excess water on the membrane surface, then pour the aqueous solution prepared in step (2) into the ultrafiltration base membrane for 2 minutes.
[0066] (5) The membrane sheet treated in step (4) is then transferred to another membrane-making tool, and the organic phase solution prepared in step (3) is poured into it for interfacial polymerization. The dipping time is 2 minutes.
[0067] (6) The membrane sheet treated in step (5) is taken out, placed in an oven for heat treatment at 70° C. for 10 min, and finally immersed in deionized water for rinsing to obtain the high-flux anti-pollution composite membrane.
[0068] Comparative Example 1
[0069] A conventional method for preparing a composite membrane, the preparation steps are as follows:
[0070] (1) 16 wt% of polymer resin is added to N,N-dimethylacetamide (DMAc) to dissolve, and 5 wt% of porogen is added, and the mixture is stirred and dissolved at 60°C, and then filtered and allowed to stand for degassing to obtain a uniform and stable polymer resin casting solution. The prepared casting solution is then vacuum degassed and coated on a non-woven fabric substrate, which is then immersed in a coagulation bath for phase inversion to obtain a wet porous ultrafiltration base membrane.
[0071] (2) Preparation of aqueous phase solution: Add 0.2 wt % of piperazine into deionized water to prepare an aqueous phase solution.
[0072] (3) Preparation of oil phase solution: 0.1 wt % of trimesoyl chloride was dissolved in an organic solvent, ISOPAR G, to prepare an oil phase solution.
[0073] (4) Cut the homemade ultrafiltration base membrane into a certain size and place it in a homemade membrane-making tool to dry excess water on the membrane surface, then pour the aqueous solution prepared in step (2) into the ultrafiltration base membrane for 2 minutes.
[0074] (5) The membrane sheet processed in step (4) is then transferred to another membrane-making tool, and the oil phase solution prepared in step (3) is poured into it for interfacial polymerization. The dipping time is 2 minutes.
[0075] (6) The membrane sheet treated in step (5) is taken out, placed in an oven for heat treatment at 70° C. for 2 min, and finally placed in deionized water for soaking and rinsing to obtain the conventional composite nanofiltration membrane.
[0076] Membrane separation performance test example
[0077] The high-flux anti-pollution composite nanofiltration membranes prepared in Examples 1-4 and the conventional composite nanofiltration membranes prepared in Comparative Example 1 were tested for flux and separation performance using a flat membrane cross-flow filtration performance evaluation device. The flux and inorganic salt retention rate test method is as follows: the operating pressure is set to 0.45 MPa, the pre-pressing time is 30 min, and then the pressure is adjusted to 0.2 MPa. After stable operation for 30 min, a certain volume of filtrate is taken and the sampling time is recorded. The membrane flux F (L·m -2 ·h -1 bar -1), and the retention rate of the corresponding inorganic salts was calculated by formula (2). All data are the average of three parallel tests under the same conditions. The spiked solution for the flux test was deionized water, and the spiked solution for the inorganic salt retention rate test was 250 mg / L MgSO4, 250 mg / L CaCl2, and 250 mg / L NaCl solution.
[0078]
[0079] In formula (1), F is the water flux, in liters per square meter per hour per bar [L / (m 2 ·h·bar)]; V is the volume of permeate collected in time t, in liters (L); A is the effective membrane area, in square meters (m 2 ) ; t is the time taken to collect V volume of permeate, in hours (h).
[0080] R=(1-C p / C f ) × 100% (2)
[0081] In formula (2), R is the interception rate (%); C p is the conductivity of the permeate, in μS / cm; C f It is the conductivity of the test liquid, in μS / cm.
[0082] The flux and separation performance test data of the high-flux composite nanofiltration membranes prepared in Examples 1-4 and the conventional composite nanofiltration membranes prepared in the comparative example are shown in Table 1 below.
[0083] Membrane anti-fouling performance test example
[0084] Using a flat membrane cross-flow filtration performance evaluation device, magnesium sulfate solution was used as the initial feed solution to test the initial flux (F0) of Example 1 and Comparative Example 1; sodium alginate was used as the pollution source, and after running for 48 hours, Example 1 and Comparative Example 1 were rinsed with deionized water for 30 minutes, and the magnesium sulfate flux was tested again. The test results are shown in Table 2.
[0085] Film contact angle test example
[0086] The contact angle of Example 1 and Comparative Example 1 was measured using a contact angle goniometer. The volume of the water droplet added during the measurement was 5 μL. The collection points were located at any 5 positions of the sample, and the average value of the contact angle was finally taken. The test results are shown in Figure 1 .
[0087] Table 1
[0088]
[0089] Table 2
[0090]
[0091] It can be seen that by controlling the appropriate proportion of the new mixed water phase system and under appropriate process conditions, the prepared composite membrane can achieve a significant increase in flux and improve the removal effect of calcium ions to a certain extent; in addition, Figure 2 As shown, the water contact angle and anti-pollution test results of the embodiments and comparative examples indicate that the surface of the nanofiltration membrane prepared in the new mixed water phase system is smoother and has better anti-pollution ability.
[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-throughput anti-pollution composite nanofiltration membrane, characterized in that: The following steps are involved: (1) sequentially adding an aqueous phase monomer having a highly chemically reactive functional group, a cationic aqueous phase monomer, and a surfactant into deionized water and dispersing them uniformly to prepare an aqueous phase solution; (2) dissolving the acyl chloride monomer in an organic solvent to prepare an organic phase solution; (3) cutting the porous ultrafiltration base membrane into a certain size, placing it in a membrane-making tool, and then pouring the prepared aqueous solution into it, dipping the porous ultrafiltration base membrane for a period of time, then pouring out the remaining liquid, and using an air knife to blow away the droplets on the membrane surface to obtain a membrane sheet; (4) placing the membrane into another membrane-making tool, and then pouring the organic phase solution into it for interfacial polymerization; (5) The membrane sheet after interfacial polymerization is taken out, placed in an oven for heat treatment, and finally immersed and rinsed in deionized water to obtain a high-throughput anti-pollution composite nanofiltration membrane.
2. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (1), the aqueous solution is composed of: 0-2.0 wt% of highly chemically reactive polyamine monomers, 0.01-0.3 wt% of cationic polyamine monomers, 0.01-2.0 wt% of surfactants, and the remainder is deionized water.
3. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 2, characterized in that: The polyamine monomer with highly chemically reactive functional groups is one or more of piperazine, 2,2'-dimethylpiperazine, 2,5-dimethylpiperazine, p-phenylenediamine, o-phenylenediamine, and mesitylenetriamine; the cationic polyamine monomer is one or more of diethylenetriamine, ethylenediamine, triethylenetetramine, and polyethylenepolyamine; the reactive surfactant is one or more of camphorsulfonic acid, sodium camphorsulfonate, sodium phosphate, and disodium hydrogen phosphate.
4. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (2), in the organic phase solution, the monomer concentration of the acyl chloride monomer is 0.01-2.0wt%; the acyl chloride monomer is one or more of trimesoyl chloride, isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, glutaryl chloride, and fumaroyl chloride; and the organic solvent is one or more of n-hexane, cyclohexane, n-heptane, ISOPAR G, and ISOPAR L.
5. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (3), the porous ultrafiltration base membrane is a commercially available porous ultrafiltration membrane, which is any one of polysulfone, polyethersulfone, sulfonated polyethersulfone, polyacrylonitrile, polyvinylidene fluoride, and cellulose acetate; the average pore size of the porous ultrafiltration membrane is 0.03-0.1 μm, preferably 0.03-0.06 μm.
6. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (3), the porous ultrafiltration base membrane is prepared by the following method: Add the polymer resin to N,N-dimethylacetamide or N,N-dimethylformamide to dissolve, add a porogen, stir and dissolve at 60-90°C, filter and stand for degassing to obtain a uniform and stable casting solution; After vacuum degassing, the prepared casting solution is coated on a non-woven fabric substrate, and the coated non-woven fabric substrate is immersed in a coagulation bath at 30-70° C. for phase inversion to obtain a wet porous ultrafiltration base membrane.
7. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 6, characterized in that: In the casting solution, the polymer resin accounts for 16-20wt%, the porogen accounts for 1-12wt%, and the balance is N,N-dimethylacetamide or N,N-dimethylformamide as a solvent; the polymer resin is any one or more of polysulfone, polyethersulfone, polyacrylonitrile, polyvinylidene fluoride, and cellulose acetate; the porogen is one or more of polyethylene glycol, propanol, isopropanol, glycerol, polyvinyl pyrrolidone, and polyethylene oxide; wherein the molecular weight of polyethylene glycol is 400-8000, polyvinyl pyrrolidone includes K30, K60, K70, K80, and K90, and the molecular weight of polyethylene oxide is 40000-1200000.
8. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (3), the time for dipping the porous ultrafiltration base membrane in the aqueous solution is 0.5-30 min, preferably 1-15 min.
9. The method for preparing a high-throughput anti-pollution composite nanofiltration membrane according to claim 1, characterized in that: In step (4), the interfacial polymerization time is 0.5-20 min, preferably 0.5-5 min; In step (5), the heat treatment temperature is 40-80°C, preferably 50-70°C; the heat treatment time is 0.5-30 min, preferably 1-10 min.
10. A high-throughput anti-pollution composite nanofiltration membrane, characterized in that: The method is described in any one of claims 1 to 9.
Citation Information
Cited By
Novel diamine monomer prepared high-flux nanofiltration membrane and method thereof
CN119701657A
Preparation method of crystallization-assisted high-flux nanofiltration membrane
CN119701658A
A method for preparing a crystallization-assisted high-flux nanofiltration membrane
CN119701658B