Preparation method of intermediate valence vanadium oxide electronic phase change material
By using low-toxicity precursors and molten alkali metal halide fluxes, the problems of low synthesis efficiency and unstable properties of intermediate valence vanadium oxides in existing technologies have been solved, achieving efficient preparation of intermediate valence vanadium oxide powders and single crystals, suitable for various electronic device applications.
Patent Information
- Application Number
- CN202410923291.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing technologies make it difficult to achieve efficient, large-scale synthesis of intermediate-valence vanadium oxides, doped vanadium oxide materials, and intermediate-valence vanadium oxide single crystals in a short time through a single reaction under low-toxicity conditions. Furthermore, existing methods often lead to deviations or loss of the properties of metal insulators.
Using low-toxicity VO2, V2O5, and NaVO3 as precursors, combined with molten alkali metal halide flux, annealing is carried out under vacuum or inert atmosphere. By controlling the oxygen partial pressure and temperature, the valence state of vanadium can be precisely controlled and doped. Through the dissolution and precipitation process of alkali metal halide flux, intermediate valence state vanadium oxide powder or single crystal is prepared.
It enables the efficient preparation of high-purity intermediate-valence vanadium oxide powder and single crystals at lower reaction temperatures and in shorter time. It allows for flexible control of the electronic phase transition temperature and is suitable for applications such as strong light protection, infrared camouflage, thermochromism, and abrupt change thermistor devices.
Smart Images

Figure CN118894724A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of functional materials, sensitive resistor materials and devices, and specifically relates to a technical method for using alkali metal halides as flux to effectively prepare intermediate-valent vanadium oxide compound powders with metal-insulator phase change properties, doped vanadium oxide compound electronic phase change powders, and efficiently prepare intermediate-valent vanadium oxide compound single crystals under a precisely controlled atmosphere. Background Art
[0002] Among the many strongly correlated oxide semiconductor material systems with metal-insulator phase transition characteristics, intermediate-valence vanadium oxide compounds have rich electronic phase structures, wide range of phase transition temperature control and high resistivity mutation degree characteristics, and have potential application value in mutation thermistors, strongly correlated logic devices, strong light protection, thermochromism, infrared camouflage, etc. [1-3]. The vanadium element in the intermediate-valence vanadium oxide compound can present a rich valence state between +3 and +5, forming V2O3, V n O 2n-1 (3≤n≤9) Magnéli, VO2, V n O 2n+1 (n≥2) Wadsley phase and other abundant binary vanadium oxide compounds; most intermediate valence vanadium oxide compounds have characteristic temperature-triggered metal-insulator phase transition characteristics, accompanied by a resistivity change of 3-5 orders of magnitude [4], which has rich application prospects in the fields of sensitive resistor devices.
[0003] The valence state of vanadium in V2O3 is +3. It transforms from a low-temperature insulator phase to a high-temperature metal phase around 168 K, and the resistivity decreases by 4-5 orders of magnitude [5]. By metal cation doping, such as Ti 4+ Cr 3+ , Fe 3+ etc., the phase transition temperature of V2O3 can be flexibly adjusted in the range of 100-200 K [6]. When doped with metal cations of the same valence, it has a dual metal-insulator phase transition triggered by different temperatures, that is, a transition from a low-temperature insulator phase to a high-temperature metal phase occurs around 160 K, and a transition from a low-temperature metal phase to a high-temperature insulator phase occurs at 350-380 K [7]; by changing the type and concentration of doped metal cations, the high-temperature phase transition temperature can be flexibly adjusted in the range of 200-460 K, making it have certain application value in the fields of positive resistance temperature coefficient thermistors, etc.
[0004] V n O 2n-1 (3≤n≤9) The valence state of vanadium in the Magnelli phase is between +3 and +4, except for V7O 13 In addition, the rest of V n O 2n-1All of them undergo a transition from a low-temperature insulator phase to a high-temperature metallic phase, with a phase transition temperature ranging from 70 K to 430 K, accompanied by a resistivity change of 1-3 orders of magnitude [8]. n O 2n-1 Among them, V3O5 is the only component known to have a phase transition temperature above room temperature, and the phase transition temperatures of the remaining components are between 70 K and 250 K [9]. Through metal cation doping, the phase transition temperature can be continuously controlled in a wide range of 40-450 K. Therefore, this system material has considerable application value in the preparation of low-temperature abrupt thermistors.
[0005] V n O 2n+1 (n≥2) The valence state of vanadium in the Wodsley phase is between +4 and +5, where V6O 13 It is the only oxide in the Wodzley phase that is known to undergo a metal-insulator transition. It transforms from a low-temperature insulator phase to a high-temperature metal phase at 150 K, accompanied by a 3-4 order of magnitude resistivity jump
[10] . The crystal structure of Wodzley phase vanadium oxides contains VO6 octahedral tubes, which are conducive to the reversible insertion of metal ions and can be used in ion battery electrodes to achieve high energy density and cycle stability
[11] .
[0006] At present, the commonly used method for synthesizing intermediate-valent vanadium oxide compounds is the solid-phase reaction method, the main process of which is to use highly toxic V2O3 and V2O5 as raw materials, and to carry out long-term solid-phase reactions multiple times under vacuum atmosphere at high temperatures of 800-1000 ℃ to achieve material synthesis
[12] . In addition, researchers often use chemical vapor transport methods to use highly toxic and easily deliquescent TeCl4 to achieve the preparation of intermediate-valent vanadium oxide single crystals in a precisely controlled high vacuum atmosphere within a specific temperature range of 950-1050 ℃
[13] . It is worth noting that when there is a small deviation between the reaction temperature and the reaction oxygen pressure, the chemical dosage ratio of the final product will deviate, resulting in the weakening or disappearance of its metal insulator properties. In addition to the solid-phase reaction, the system material can also be synthesized by chemical methods, using VOCl3 as a precursor and organic substances such as benzyl alcohol as solvents, and keeping the temperature at 250 ℃ for 90 minutes to achieve material synthesis
[14] . However, the electrical and optical properties of intermediate-valent vanadium oxide compounds synthesized by chemical methods are difficult to meet the actual use standards.
[0007] In summary, the art currently lacks an effective method for mass-producing intermediate-valent vanadium oxide compounds, doped vanadium oxide compound materials, and intermediate-valent vanadium oxide compound single crystals through a single reaction at a relatively low reaction temperature in a relatively short period of time using low-toxic precursors without the aid of a reducing atmosphere.
[0008] 【1】 Ngai J H, Walker F J, Ahn C H. Correlated Oxide Physics andElectronics. Annual Review of Materials Research[J], 2014, 44: 1-17.
[0009] 【2】 Morin F J. Oxides Which Show a Metal-to-Insulator Transition atthe Neel Temperature [J]. Physical Review Letters, 1959, 3(1): 34-6.
[0010] 【3】 Kachi S, Kosuge K, Okinaka H. Metal-insulator transition in V n O 2n−1 [J]. Journal of Solid State Chemistry, 1973, 6(2): 258-70.
[0011] 【4】 Nagasawa K, Bando Y, Takada T. Growth and Electrical Propertiesof V n O 2n−1 (n=3, 4, ..., 8) Single Crystals [J]. Bulletin of the Institute forChemical Research, Kyoto University, 1972, 49(5): 322-41.
[0012] 【5】 Feinleib J, Paul W. Semiconductor-To-Metal Transition in V2O3 [J].Physical Review, 1967, 155(3): 841-50.
[0013] 【6】 McWhan D B, Remeika J P. Metal-Insulator Transition in (V 1-x Cr x)2O3[J]. Physical Review B, 1970, 2(9): 3734-50.
[0014] 【7】 Chandrashekhar G V, Shin S H, Jayaraman A, et al. Electricalproperties of (Ti x V 1–x )2O3 [J]. physica status solidi (a), 1975, 29(1): 323-9.
[0015] 【8】 Kachi S, Kosuge K, Okinaka H. Metal-insulator transition in V n O 2n−1 [J]. Journal of Solid State Chemistry, 1973, 6(2): 258-70.
[0016] 【9】Andreev V N, Klimov V A. Specific features of electricalconductivity of V3O5 single crystals [J]. Physics of the Solid State, 2011, 53(12): 2424-30.
[0017]
[10] Kawashima K, Ueda Y, Kosuge K, et al. Crystal growth and someelectric properties of V6O 13 [J]. Journal of Crystal Growth, 1974, 26(2): 321-2.
[0018]
[11] Shimizu Y, Aoyama S, Jinno T, et al. Site-Selective MottTransition in a Quasi-One-Dimensional Vanadate V6O 13 [J]. Physical ReviewLetters, 2015, 114(16).
[0019]
[12] MacChesney J B, Guggenheim H J. Growth and electrical properties of vanadium dioxide single crystals containing selected impurity ions [J]. Journal of Physics and Chemistry of Solids, 1969, 30(2): 225-34.
[0020]
[13] Okinaka H, Nagasawa K, Kosuge K, et al. Electrical Properties of the V5O9 Single Crystals [J]. Journal of the Physical Society of Japan, 1970, 28(3): 803.
[0021]
[14] Jing Xu, Chenguo Hu, Huayong Han, Mingquan He, Buyong Wan and Chuanhui Xia, "The synthesis and photoelectric response of single-crystalline V4O7 nanowires," 2010 3rd International Nanoelectronics Conference (INEC), Hong Kong, 2010, pp. 413-414. Summary of the Invention
[0022] The purpose of the present invention is to provide a method for preparing an intermediate-valent vanadium oxide electronic phase-change ceramic material; the main idea is to use metal vanadium, low-toxic VO2, V2O5, and NaVO3 powder as precursors, use molten alkali metal halide flux to fully dissolve the precursor of the system material, and generate the intermediate-valent vanadium oxide compound to be prepared during the cooling process under vacuum or inert gas atmosphere, and precipitate together with the gradually solidified alkali metal halide molten salt. Compared with the previous synthesis method of the system material, the advantage of the technology provided by the present invention is that it uses low-toxic precursors and molten alkali metal halide flux, does not rely on reducing atmosphere, greatly reduces the material synthesis temperature, shortens the reaction time, and realizes flexible regulation of the valence of the vanadium element in the intermediate-valent vanadium oxide compound, so as to achieve the large-scale preparation of the material system powder and the efficient growth of the material system single crystal. By adjusting the ratio of high- and low-valence precursors of vanadium elements and the types and ratios of doped transition metal oxides, the composition and crystal structure of the prepared intermediate-valence vanadium oxide compounds can be accurately controlled, and further the wide range of adjustment of the metal insulator phase change characteristics and electrical transport relationship can be achieved. The prepared materials have application value in the fields of positive and negative resistance temperature coefficient mutation thermistors, strong light protection, thermochromism and infrared camouflage.
[0023] A method for preparing an intermediate valence vanadium oxide electronic phase change material, characterized in that a synthesis method is provided to achieve the growth of a vanadium oxide material having an intermediate valence vanadium element, and simultaneously introduce a doping element; the preparation method can synthesize VO2, Magnelli phase V n O 2n-1 (3≤n≤9), V2O3, Wodsley phase V n O 2n+1 (3≤n≤9); by coordinating the valence state regulation of vanadium elements and doping with transition metal elements, the electronic phase transition temperature can be continuously regulated in a wide range of 40-450 K. The method comprises the following steps:
[0024] 1) According to the electronic phase transition characteristics of the metal insulator to be achieved, select vanadium elements and oxides with higher and lower valence states than the vanadium element in the target intermediate valence vanadium oxide as precursors, such as metal vanadium powder, low-toxic VO2, V2O5 and NaVO3, and add doped metal oxides. According to the principles of conservation of element mass before and after synthesis and conservation of element electron transfer, the molar ratio of the vanadium-containing precursor and the doped metal oxide is determined, and the mixture is weighed and fully mixed.
[0025] 2) Add a flux with a certain melting point according to the temperature of the subsequent solid phase reaction to be used, and add the selected flux to the above-mentioned precursor mixed powder in a certain proportion, and mix again to be uniform.
[0026] 3) Adopting an annealing process under a certain atmosphere, the precursor to which an alkali metal halide flux is added is first rapidly heated to above the melting point of the flux at a heating rate of 10 °C / min in a vacuum or inert atmosphere with an oxygen partial pressure precisely controlled within a certain range, so that the precursor is fully dissolved in the molten flux, thereby ensuring the precise control of the valence state of the vanadium element in the intermediate-valence vanadium oxide compound to be fitted; then the temperature is slowly lowered to below the melting point of the flux, and after being kept warm for a period of time, it is cooled to room temperature at a set cooling rate; the alkali metal halide flux in the obtained powder product is removed by water washing, thereby obtaining an intermediate-valence vanadium oxide powder or single crystal; the obtained powder is further cold pressed and sintered to obtain an intermediate-valence vanadium oxide ceramic.
[0027] Furthermore, step 1) by regulating the valence state of vanadium in the intermediate valence vanadium oxide compound and combining the substitution of the main group metal element or the transition group metal element for the vanadium element, the trigger temperature of the metal insulator phase transition characteristic of the material can be regulated in the range of 40-450 K; wherein the valence state of the vanadium element can be controlled by metal vanadium powder, VO2, V2O5 and NaVO3, including the following components: V2O3, V3O5, V4O7, V5O9, V6O 11 , VO2, V6O 13 ; Transition group elements mainly include Cr, Ti, Mo, Fe, W, Nb, and Zr.
[0028] Furthermore, in the synthesis of V2O3, the transition group doping elements are preferably Cr, Ti, Mo, Fe, and Zr, and the main group doping elements are preferably Al, Ga, and In; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V2O3, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at high temperature, thereby accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -10 -10 -8In a vacuum or inert atmosphere precisely controlled within the Pa range, by keeping warm at 800-900 ℃ for 24 hours and cooling to room temperature at a cooling rate of 2-5 ℃ / min, V2O3 pure phase powder can be obtained; when the doped metal elements are Cr, Al, Ga, In and other doped elements with the same valence, the doped V2O3 has a metal-insulator phase transition triggered by different characteristic temperatures, that is, a transition from a low-temperature insulator phase to a high-temperature metal phase occurs near 170 K, and a transition from a low-temperature metal phase to a high-temperature insulator phase occurs near 380 K.
[0029] Furthermore, in the synthesis of the intermediate valence vanadium oxide compound V3O5 of the Magnelli phase, the transition group doping elements are preferably Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V3O5, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at high temperature, thereby accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -8 -10 -7 V3O5 pure phase powder can be obtained by keeping the temperature at 820-920 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
[0030] Furthermore, in the synthesis of the intermediate valence vanadium oxide compound V4O7 of the Magnelli phase, the transition group doping elements are preferably Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V4O7, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at high temperature, thereby accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -7 -10 -6V4O7 pure phase powder can be obtained by keeping the temperature at 830-930 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
[0031] Furthermore, in the synthesis of the intermediate valence vanadium oxide compound V5O9 of the Magnelli phase, the transition group doping elements are preferably Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V5O9, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at high temperature, thereby accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -6 -10 -5 V5O9 pure phase powder can be obtained by keeping the temperature at 840-940 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
[0032] Furthermore, the intermediate valence vanadium oxide V6O in the Magnelli phase was synthesized. 11 In the process, the transition doping elements are preferably Cr, Ti, Mo, Nb, and Fe; the fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than that of the synthetic V6O 11 The required melting point and the ability to dissolve the precursor powder in a high temperature liquid state can make the precursor powder evenly dispersed in the flux at high temperature, thus accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -5 -10 -4 V6O can be obtained by keeping the temperature at 850-950 °C for 24 hours in a vacuum or inert atmosphere precisely controlled within the range of Pa and cooling to room temperature at a cooling rate of 2-5 °C / min. 11 Pure phase powder.
[0033] Furthermore, in the synthesis of doped VO2, the transition doping elements are preferably Cr, Ti, Mo, Fe, W, and Nb; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of doped VO2, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at high temperature, thereby accelerating the reaction rate. The mixture of the synthetic material precursor and the flux should be prepared at an oxygen partial pressure of 10 -4 -10 -2 In a vacuum or inert atmosphere precisely controlled within the Pa range, the doped VO2 pure phase powder can be obtained by keeping the temperature at 850-950 °C for 24 hours and cooling it to room temperature at a cooling rate of 2-5 °C / min. By adjusting the type and proportion of transition group doping elements, the metal-insulator phase transition temperature of VO2 can be flexibly controlled within the temperature range of 100-400 K.
[0034] Furthermore, the intermediate valence vanadium oxide V6O in the Wodzley phase was synthesized. 13 In the process, the transition doping elements are preferably Cr, Ti, Nb and Mo; the fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, NaCl and LiCl and other fluxes can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than that of the synthetic V6O 13 The required melting point and the ability to dissolve the precursor powder in a high temperature liquid state can make the precursor powder evenly dispersed in the flux at high temperature, thus accelerating the reaction rate. The mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -5 -10 -3 V6O can be obtained by keeping the temperature at 650-750 °C for 24 hours in a vacuum or inert atmosphere precisely controlled within the range of Pa and cooling to room temperature at a cooling rate of 5 °C / min. 13 Pure phase powder.
[0035] Furthermore, in the synthesis of intermediate-valent vanadium oxide, by controlling the cooling rate, the grain size of the material can be flexibly controlled; if the temperature is slowly cooled from a certain reaction temperature to room temperature at a cooling rate of 0.01-1 ℃ / min, an intermediate-valent vanadium oxide single crystal grown along a specific crystal direction is finally synthesized, and its grain size range is 1-5 mm; if the temperature is slowly cooled from a certain reaction temperature to room temperature at a cooling rate of 2-5 ℃ / min, a pure-phase powder of intermediate-valent vanadium oxide is finally synthesized, and its grain size range is 30-50 μm; if water is used as a coolant, from a certain reaction temperature, it is extremely quickly cooled to room temperature by quenching, and a pure-phase powder with a grain size range of 5-10 μm can be obtained.
[0036] The present invention proposes a method for mass-producing electronic phase change powder, ceramic material and single crystal of an intermediate-valent vanadium oxide compound. Compared with other methods, the advantage of this method is that the precursors required for the synthesis of the system materials are fully dissolved by means of a molten alkali metal halide flux. During this process, the precursors fully react, which greatly reduces the reaction temperature and reaction time required for the synthesis of the materials. The method can realize the mass-production of high-purity and high-uniformity polycrystalline or single-crystalline materials under a precisely controlled atmosphere. By further regulating the valence state of the vanadium element in the intermediate-valent vanadium oxide compound, the type of doping elements and the doping ratio, the metal-insulator transition temperature of the material can be continuously regulated within a wide range. The method has certain application prospects in the fields of strong light protection, infrared camouflage, thermochromism and sudden thermistor devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is an X-ray diffraction diagram of V2O3 powder prepared by the flux method proposed in the present invention. It can be seen that the prepared powder is a pure phase powder.
[0038] Figure 2 For the (V) prepared by the flux method proposed by the present invention 0.99 Cr 0.01 )2O3 powder material's X-ray diffraction pattern shows that the prepared powder is a pure phase powder.
[0039] Figure 3 For the (V) prepared by the flux method proposed by the present invention 0.99 Cr 0.01 )2O3 powder material resistivity versus temperature. The material undergoes two metal-insulator phase transitions. The low-temperature insulator phase transitions to the high-temperature metal phase at a phase transition temperature of 168 K and the low-temperature metal phase transitions to the high-temperature insulator phase at a phase transition temperature of 400 K.
[0040] Figure 4This is an X-ray diffraction diagram of V3O5 powder prepared by the flux method proposed in the present invention. It can be seen that the prepared powder is a pure phase powder.
[0041] Figure 5 The figure is a relationship between the resistivity and temperature of the V3O5 powder material prepared by the flux method proposed in the present invention. The material undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase at a phase transition temperature of 428 K. DETAILED DESCRIPTION
[0042] Unless otherwise specified, the various raw materials used in the present invention can be obtained from the market or prepared according to conventional methods in the art. Unless otherwise defined or specified, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.
[0043] Other aspects of the present invention will be apparent to those skilled in the art in view of the disclosure herein.
[0044] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0045] Example 1: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground evenly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and VO2 and metal V powder were mixed evenly. The mixture was ground evenly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the Pa range, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0046] Example 2: V, VO2, and Cr2O3 were weighed in a molar ratio of V: VO2: Cr2O3 = 1.485:0.495:0.01, and were placed in an agate mortar and ground thoroughly. Then, KCl with a molar ratio of VO2: KCl = 1:10 was weighed, and VO2 and metal V powder were mixed and ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 Pa range, first sintered at 900 ° C for 30 minutes, then kept at 800 ° C for 24 hours, and cooled to room temperature at a cooling rate of 5 ° C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase (V 0.99 Cr 0.01 )2O3 powder, a binder is added to the obtained powder, cold pressed and sintered to obtain the ceramic material of this component. The low-temperature insulator phase transitions to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered is 100 times; the low-temperature metal phase transitions to the high-temperature insulator phase near 400 K, and the resistivity mutation degree triggered is 3 times.
[0047] Example 3: V, VO2, and In2O3 were weighed in a molar ratio of V: VO2: In2O3 = 1.485: 0.495: 0.01, and were placed in an agate mortar and ground thoroughly. Then, KCl with a molar ratio of VO2: KCl = 1:10 was weighed, and VO2 and metal V powders were mixed and ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 Pa range, first sintered at 900 ° C for 30 minutes, then kept at 800 ° C for 24 hours, and cooled to room temperature at a cooling rate of 5 ° C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase (V 0.99 In 0.01 )2O3 powder, a binder is added to the obtained powder, cold pressed and sintered to obtain the ceramic material of this component. At the phase transition characteristic temperature of 170 K, a transition from low-temperature insulator phase to high-temperature metal phase occurs, and the resistivity mutation degree triggered is 200 times; at around 380 K, a transition from low-temperature metal phase to high-temperature insulator phase occurs, and the resistivity mutation degree triggered is 5 times.
[0048] Example 4: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground evenly. Then, NaCl at a molar ratio of VO2: NaCl = 1:10 was weighed, and VO2 and metal V powder were mixed evenly. The mixture was ground evenly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 950 °C for 30 minutes, then kept at 850 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0049] Example 5: V and V2O5 were weighed at a molar ratio of V:V2O5=4:3, and were placed in an agate mortar and ground evenly. Then, NaCl at a molar ratio of V2O5:NaCl=1:10 was weighed, and the mixed VO2 and V2O5 powders were added. The mixture was ground evenly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 950 °C for 30 minutes, then kept at 850 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0050] Example 6: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground evenly. Then, NaCl and KCl were weighed at a molar ratio of VO2: NaCl: KCl = 1:10:10, and VO2 and metal V powder were mixed evenly. The mixture was ground evenly again, and the mixture was cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 800 °C for 30 minutes, then kept at 700 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0051] Example 7: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground evenly. Then, CsI was weighed at a molar ratio of VO2: CsI = 1:10, and VO2 and metal V powder were mixed evenly. The mixture was ground evenly again, and a block with a diameter of 10 mm was cold pressed by a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the Pa range, the samples were first sintered at 650 °C for 30 minutes, then kept at 600 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0052] Example 8: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground evenly. Then, KI and RbI were weighed at a molar ratio of VO2: KI: RbI = 1:2:1, and VO2 and metal V powder were mixed evenly. The mixture was ground evenly again, and the mixture was cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 700 °C for 30 minutes, then kept at 630 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0053] Example 9: V and VO2 were weighed at a molar ratio of V: VO2 = 2.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -8 -10 -7 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V3O5 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase at the phase transition characteristic temperature of 420 K, and the resistivity mutation degree triggered was 10 times.
[0054] Example 10: V and VO2 were weighed at a molar ratio of V: VO2 = 3.5:0.5, and were placed in an agate mortar and ground evenly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground evenly again, and the mixture was cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -7 -10 -6 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the sample was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V4O7 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. A transition from a low-temperature insulator phase to a high-temperature metal phase occurred near the phase transition characteristic temperature of 250 K, and the resistivity mutation degree triggered was 100 times.
[0055] Example 11: V and VO2 were weighed at a molar ratio of V: VO2 = 4.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the VO2 and metal V powders were mixed and ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -6 -10 -5In a vacuum or inert atmosphere precisely controlled within the Pa range, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V5O9 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. A transition from a low-temperature insulator phase to a high-temperature metal phase occurred near the phase transition characteristic temperature of 130 K, and the resistivity mutation degree triggered was 200 times.
[0056] Example 12: V and VO2 were weighed at a molar ratio of V: VO2 = 5.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the VO2 and metal V powders were mixed and ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -4 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction was completed. Finally, the powder sample was rinsed with deionized water and dried to obtain pure V6O 11 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component, which undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase near the phase transition characteristic temperature of 170 K, and the resistivity mutation degree triggered is 10 times.
[0057] Example 13: VO2 and TiO2 were weighed at a molar ratio of VO2:TiO2=0.95:0.05, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and the mixed VO2 and TiO2 powders were added. The mixture was ground thoroughly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction was completed. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V 0.95 Ti 0.05 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase transition to a high-temperature metal phase occurs near the phase transition characteristic temperature of 320 K, and the resistivity mutation degree triggered is 100 times.
[0058] Example 14: VO2 and Cr2O3 were weighed at a molar ratio of VO2:Cr2O3=0.95:0.05, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and the mixed VO2 and Cr2O3 powders were added. The mixture was ground thoroughly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the powder was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V 0.9 Cr 0.1 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase to a high-temperature metal phase transition occurs near the phase transition characteristic temperature of 360 K, and the resistivity mutation degree triggered is 10 times.
[0059] Example 15: VO2 and WO3 were weighed at a molar ratio of VO2:WO3 = 0.99:0.01, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl = 1:10 was weighed, and the mixed VO2 and WO3 powders were added, and the mixture was ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the powder was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V 0.99 W 0.01 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase to a high-temperature metal phase transition occurs near the phase transition characteristic temperature of 300 K, and the resistivity mutation degree triggered is 10 times.
[0060] Example 16: VO2 and Nb2O5 were weighed at a molar ratio of VO2:Nb2O5=0.95:0.05, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and the mixed VO2 and Nb2O5 powders were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3In a vacuum or inert atmosphere precisely controlled within the range of Pa, the powder was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V 0.9 Nb 0.1 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase to a high-temperature metal phase transition occurs near the phase transition characteristic temperature of 300 K, and the resistivity mutation degree triggered is 10 times.
[0061] Example 17: V and V2O5 were weighed at a molar ratio of V2O5:V=26:4, and were placed in an agate mortar and ground evenly. Then, KCl at a molar ratio of V2O5:KCl=1:10 was weighed, and the mixed V2O5 and metal V powder were added. The mixture was ground evenly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction was completed. Finally, the powder sample was rinsed with deionized water and dried to obtain pure V6O 13 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component, which undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase near the phase transition characteristic temperature of 150 K, and the resistivity mutation degree triggered is 100 times.
[0062] Example 18: VO2 and V2O5 were weighed at a molar ratio of V2O5:VO2 = 1:4, and were placed in an agate mortar and ground evenly. Then, KCl at a molar ratio of VO2:KCl = 1:10 was weighed, and the mixed V2O5 and VO2 powders were added. The mixture was ground evenly again, and cold-pressed into blocks with a diameter of 10 mm using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction was completed. Finally, the powder sample was rinsed with deionized water and dried to obtain pure V6O 13 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component, which undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase near the phase transition characteristic temperature of 150 K, and the resistivity mutation degree triggered is 100 times.
[0063] Example 19: VO2 and V2O5 were weighed at a molar ratio of V2O5:VO2 = 1:4, and were placed in an agate mortar and ground evenly. Then, NaCl and KCl were weighed at a molar ratio of VO2:NaCl:KCl = 1:10:10, and the mixed V2O5 and VO2 powders were added. The mixture was ground evenly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 800 °C for 30 minutes, then kept at 700 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction was completed. Finally, the powder sample was rinsed with deionized water and dried to obtain pure V6O 13 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component, which undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase near the phase transition characteristic temperature of 150 K, and the resistivity mutation degree triggered is 100 times.
[0064] Example 20: V and VO2 were weighed at a molar ratio of V: VO2 = 1.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the Pa range, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 0.1 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V2O3 single crystal with a size of about 2 mm. The low-temperature insulator phase transformed to the high-temperature metal phase at the phase transition characteristic temperature of 168 K, and the resistivity mutation triggered by it was 10,000 times.
[0065] Example 21: V and VO2 were weighed at a molar ratio of V: VO2 = 2.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -8 -10 -7In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 0.1 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V3O5 single crystal with a size of about 3 mm. The low-temperature insulator phase transformed to the high-temperature metal phase at the phase transition characteristic temperature of 420 K, and the resistivity mutation triggered by it was 100 times.
[0066] Example 22: V and VO2 were weighed at a molar ratio of V: VO2 = 3.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -7 -10 -6 In a vacuum or inert atmosphere precisely controlled within the Pa range, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 0.1 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V4O7 single crystal with a size of about 2.5 mm. The low-temperature insulator phase transformed to the high-temperature metal phase at a phase transition characteristic temperature of 250 K, triggering a 1000-fold increase in resistivity.
[0067] Example 23: V and VO2 were weighed at a molar ratio of V: VO2 = 4.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -6 -10 -5 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 0.1 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V5O9 single crystal with a size of about 3 mm. The low-temperature insulator phase transformed to the high-temperature metal phase at the phase transition characteristic temperature of 130 K, and the resistivity mutation triggered was 2000 times.
[0068] Example 24: V and VO2 were weighed at a molar ratio of V: VO2 = 5.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -4 In a vacuum or inert atmosphere precisely controlled within the Pa range, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 0.1 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V6O with a size of about 2 mm. 11 For single crystals, a transition from a low-temperature insulator phase to a high-temperature metal phase occurs near the phase transition characteristic temperature of 170 K, and the resistivity mutation degree triggered is 100 times.
[0069] Example 25: V and VO2 were weighed at a molar ratio of V: VO2 = 2.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -8 -10 -7 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V3O5 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 420 K, and the resistivity mutation degree triggered was 10 times.
[0070] Example 26: V and VO2 were weighed at a molar ratio of V: VO2 = 3.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -7 -10 -6In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction was completed, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V4O7 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. A low-temperature insulator phase transformed into a high-temperature metal phase near the phase transition characteristic temperature of 250 K, and the resistivity mutation degree triggered was 100 times.
[0071] Example 27: V and VO2 were weighed at a molar ratio of V: VO2 = 4.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -6 -10 -5 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction was completed, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain a pure phase V5O9 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain a ceramic material of this component. A low-temperature insulator phase transformed into a high-temperature metal phase near the phase transition characteristic temperature of 130 K, and the resistivity mutation degree triggered was 200 times.
[0072] Example 28: V and VO2 were weighed at a molar ratio of V: VO2 = 5.5:0.5, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2: KCl = 1:10 was weighed, and the mixed VO2 and metal V powder were added. The mixture was ground thoroughly again, and the blocks were cold pressed into a 10 mm diameter block using a press. The blocks were then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -5 -10 -4 In a vacuum or inert atmosphere precisely controlled within the Pa range, the reaction was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction was completed, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain pure V6O 11 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component, which undergoes a phase transition from a low-temperature insulator phase to a high-temperature metal phase near the phase transition characteristic temperature of 170 K, and the resistivity mutation degree triggered is 10 times.
[0073] Example 29: VO2 and TiO2 were weighed at a molar ratio of VO2:TiO2=0.95:0.05, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and the mixed VO2 and TiO2 powders were added. The mixture was ground thoroughly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3 In a vacuum or inert atmosphere precisely controlled within the Pa range, the sample was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction was completed, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V. 0.95 Ti 0.05 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase transition to a high-temperature metal phase occurs near the phase transition characteristic temperature of 320 K, and the resistivity mutation degree triggered is 100 times.
[0074] Example 30: VO2 and Cr2O3 were weighed at a molar ratio of VO2:Cr2O3=0.95:0.05, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and the mixed VO2 and Cr2O3 powders were added. The mixture was ground thoroughly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the sample was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V. 0.9 Cr 0.1 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase to a high-temperature metal phase transition occurs near the phase transition characteristic temperature of 360 K, and the resistivity mutation degree triggered is 10 times.
[0075] Example 31: VO2 and WO3 were weighed at a molar ratio of VO2:WO3 = 0.99:0.01, and were placed in an agate mortar and ground thoroughly. Then, KCl at a molar ratio of VO2:KCl = 1:10 was weighed, and the mixed VO2 and WO3 powders were added, and the mixture was ground thoroughly again. The blocks were cold pressed into a 10 mm diameter block using a press, and then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -4 -10 -3In a vacuum or inert atmosphere precisely controlled within the range of Pa, the sample was first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours. After the reaction, water was used as a coolant to quench and cool to room temperature. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V. 0.99 W 0.01 O2 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, a low-temperature insulator phase to a high-temperature metal phase transition occurs near the phase transition characteristic temperature of 300 K, and the resistivity mutation degree triggered is 20 times.
[0076] Example 32: V and NaVO3 were weighed at a molar ratio of V:NaVO3=2:3, and were placed in an agate mortar and ground evenly. Then, KCl at a molar ratio of VO2:KCl=1:10 was weighed, and NaVO3 and metal V powder were mixed evenly. The mixture was ground evenly again, and cold-pressed into a block with a diameter of 10 mm using a press. The block was then placed in an alumina crucible and placed in an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the range of Pa, the samples were first sintered at 900 °C for 30 minutes, then kept at 800 °C for 24 hours, and cooled to room temperature at a cooling rate of 5 °C / min after the reaction. Finally, the powder sample was rinsed with deionized water and dried to obtain pure phase V2O3 powder. A binder was added to the obtained powder, cold pressed, and then sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 168 K, and the resistivity mutation degree triggered was 100 times.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the substantial technical content of the present invention. The substantial technical content of the present invention is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.
Claims
1. A method for preparing an intermediate valence vanadium oxide electronic phase change material, characterized in that Provide a synthesis method to achieve the growth of vanadium oxide materials with intermediate valence vanadium elements and introduce doping elements at the same time; the preparation method can synthesize VO2, Magnelli phase V n O 2n-1 (3≤n≤9), V2O3, Wodsley phase V n O 2n+1 (3≤n≤9); by coordinating the valence state regulation of vanadium elements and doping with transition metal elements, the electronic phase transition temperature can be continuously regulated in a wide range of 40-450 K; the method comprises the following steps: 1) According to the electronic phase transition characteristics of the metal insulator to be achieved, select vanadium elements and oxides with higher and lower valence states than the vanadium element in the target intermediate valence vanadium oxide as precursors, including metal vanadium powder, low-toxic VO2, V2O5 and NaVO3, and add doped metal oxides, and determine the amount ratio of the vanadium-containing precursor and the doped metal oxide based on the principles of element mass conservation before and after synthesis and element electron transfer conservation, weigh and fully mix; 2) Add a flux with a certain melting point according to the temperature of the subsequent solid phase reaction to be used, and add the selected flux to the above-mentioned precursor mixed powder in a certain proportion, and mix again; 3) Adopting an annealing process under a certain atmosphere, the precursor to which an alkali metal halide flux is added is first rapidly heated to above the melting point of the flux at a heating rate of 10 °C / min in a vacuum or inert atmosphere with an oxygen partial pressure precisely controlled within a certain range, so that the precursor is fully dissolved in the molten flux, thereby ensuring the precise control of the valence state of the vanadium element in the intermediate-valence vanadium oxide compound to be fitted; then the temperature is slowly lowered to below the melting point of the flux, and after being kept warm for a period of time, it is cooled to room temperature at a set cooling rate; the alkali metal halide flux in the obtained powder product is removed by water washing, thereby obtaining an intermediate-valence vanadium oxide powder or single crystal; the obtained powder is further cold pressed and sintered to obtain an intermediate-valence vanadium oxide ceramic.
2. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 1, characterized in that: Step 1) By regulating the valence state of vanadium in the intermediate valence vanadium oxide compound and combining the substitution of main group metal elements or transition group metal elements for vanadium, the trigger temperature of the metal insulator phase transition characteristic of the material can be regulated in the range of 40-450 K; wherein, the valence state of vanadium can be controlled by metal vanadium powder, VO2, V2O5 and NaVO3, including the following components: V2O3, V3O5, V4O7, V5O9, V6O 11 , VO2, V6O 13 ; Transition group elements mainly include Cr, Ti, Mo, Fe, W, Nb, and Zr.
3. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: In the synthesis of V2O3, transition group doping elements include Cr, Ti, Mo, Fe, and Zr, and main group doping elements include Al, Ga, and In; fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of a new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of a new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V2O3, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is evenly dispersed in the flux at a high temperature, thereby accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -10 -10 -8 In a vacuum or inert atmosphere precisely controlled within the Pa range, by keeping warm at 800-900 ℃ for 24 hours and cooling to room temperature at a cooling rate of 2-5 ℃ / min, V2O3 pure phase powder can be obtained; when the doped metal elements are Cr, Al, Ga, and In doped elements of the same valence state, there is a metal-insulator phase transition triggered by different characteristic temperatures in the doped V2O3, that is, a transition from a low-temperature insulator phase to a high-temperature metal phase occurs near 170 K, and a transition from a low-temperature metal phase to a high-temperature insulator phase occurs near 380 K.
4. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: In the synthesis of the intermediate valence vanadium oxide compound V3O5 of the Magnelli phase, the transition group doping elements include Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V3O5, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is uniformly dispersed in the flux at a high temperature, thereby accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -8 -10 -7 V3O5 pure phase powder can be obtained by keeping the temperature at 820-920 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
5. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: In the synthesis of the intermediate valence vanadium oxide compound V4O7 of the Magnelli phase, the transition group doping elements include Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V4O7, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is uniformly dispersed in the flux at a high temperature, thereby accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -7 -10 -6 V4O7 pure phase powder can be obtained by keeping the temperature at 830-930 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
6. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: In the synthesis of the intermediate valence vanadium oxide compound V5O9 of the Magnelli phase, the transition group doping elements include Cr, Ti, Mo, Nb, and Fe; the flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of V5O9, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder is uniformly dispersed in the flux at a high temperature, thereby accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -6 -10 -5 V5O9 pure phase powder can be obtained by keeping the temperature at 840-940 ℃ for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 ℃ / min.
7. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: Synthesis of Magnelli Phase Intervalent Vanadium Oxide V6O 11 In the process, the transition doping elements include Cr, Ti, Mo, Nb, and Fe; the fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase. The melting point of the flux is required to be lower than that of the synthetic V6O 11 The required melting point and the ability to dissolve the precursor powder in a high temperature liquid state, so that the precursor powder can be evenly dispersed in the flux at a high temperature, accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -5 -10 -4 V6O can be obtained by keeping the temperature at 850-950 °C for 24 hours in a vacuum or inert atmosphere precisely controlled within the range of Pa and cooling to room temperature at a cooling rate of 2-5 °C / min. 11 Pure phase powder.
8. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: In the synthesis of doped VO2, the transition doping elements include Cr, Ti, Mo, Fe, W, and Nb; the fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase; the melting point of the flux is required to be lower than the melting point required for the synthesis of doped VO2, and it can dissolve the precursor powder in a high-temperature liquid state, so that the precursor powder can be evenly dispersed in the flux at high temperature to accelerate the reaction rate; the mixture of the synthetic material precursor and the flux should be heated at an oxygen partial pressure of 10 -4 -10 -2 By keeping the temperature at 850-950 °C for 24 hours in a vacuum or inert atmosphere precisely controlled within the Pa range and cooling to room temperature at a cooling rate of 2-5 °C / min, doped VO2 pure phase powder can be obtained; by adjusting the type and proportion of transition group doping elements, the metal-insulator phase transition temperature of VO2 can be flexibly controlled in the temperature range of 100-400 K.
9. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 2, characterized in that: Synthesis of Wodsley Phase Intervalent Vanadium Oxide V6O 13 In the process, the transition doping elements include Cr, Ti, Nb, and Mo; the fluxes include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI. A single flux can be used to assist the growth of the new phase, or a mixture of KCl and RbCl, KCl and NaCl, CsCl and LiBr, KCl and LiCl, and NaCl and LiCl can be used to assist the growth of the new phase. The melting point of the flux is required to be lower than that of the synthetic V6O 13 The required melting point and the ability to dissolve the precursor powder in a high temperature liquid state, so that the precursor powder can be evenly dispersed in the flux at a high temperature, accelerating the reaction rate; the mixture of the material precursor and the flux should be prepared at an oxygen partial pressure of 10 -5 -10 -3 V6O can be obtained by keeping the temperature at 650-750 °C for 24 hours in a vacuum or inert atmosphere precisely controlled within the range of Pa and cooling to room temperature at a cooling rate of 5 °C / min. 13 Pure phase powder.
10. The method for preparing an intermediate valence vanadium oxide electronic phase change material according to claim 1, characterized in that: In step 3), in the synthesis of intermediate-valent vanadium oxide, by controlling the cooling rate, the grain size of the material can be flexibly controlled; if the temperature is slowly cooled from a certain reaction temperature to room temperature at a cooling rate of 0.01-1 °C / min, an intermediate-valent vanadium oxide single crystal grown along a specific crystal direction is finally synthesized, and its grain size range is 1-5 mm; if the temperature is slowly cooled from a certain reaction temperature to room temperature at a cooling rate of 2-5 °C / min, a pure phase powder of intermediate-valent vanadium oxide is finally synthesized, and its grain size range is 30-50 μm; if water is used as a coolant, from a certain reaction temperature, it is extremely quickly cooled to room temperature by quenching, and a pure phase powder with a grain size range of 5-10 μm can be obtained.
Citation Information
Patent Citations
Near-room-temperature phase-changing vanadium oxide nano material and preparation method thereof
CN107915258A
Method for preparing electronic phase change ceramic material by doping vanadium oxide with transition metal oxide
CN114538924A
Preparation method of high-strength and high-stability vanadium oxide electronic phase change composite ceramic
CN114538925A
Preparation method of rare earth alkaline earth manganese-based perovskite electronic phase change ceramic material
CN116903369A
Rare earth bismuth nickel-based layered perovskite oxide electronic phase change material and preparation method thereof
CN118005094A
Cited By
Molten salt assisted oxygen partial pressure self-adjusting intermediate valence transition group oxide preparation method
CN121449099A
A covering agent for gallium antimonide surface growth and a preparation method thereof
CN122707237A
A covering agent for gallium antimonide surface growth and a preparation method thereof
CN122707237B