Pressure-bearing plugging material for malignant leakage of fractured formation, drilling fluid and application
By using high-dehydration composite leak plugging agents and fill cementing agents of diatomaceous earth, ultrafine calcium carbonate, mica sheets and other materials, combined with active agents and dispersants, a sealed plugging layer is formed, which solves the leakage of drilling fluid in crack formations. The problem is that efficient blockage and long-term stable blocking effect are achieved, reducing reservoir damage.
Patent Information
- Application Number
- CN202310492626.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-04
AI Technical Summary
During the drilling process of crack formations, the drilling fluid leakage frequency is high and the leakage volume is large. The existing leakage plugging technology is difficult to effectively match the formation cracks, resulting in the sealing material being easily damaged under high temperature and high pressure, the re-leakage frequency is high, and it is difficult to unblock the blocking material. , causing reservoir damage.
Use high-dehydration composite leak plugging agent composed of diatomaceous earth, ultrafine calcium carbonate, mica sheets, etc., and a filling cementitious agent combining white asphalt, asbestos fiber and sodium silicate, and an active agent of heavy calcium carbonate and silica fume powder. , and dispersants of humate and polycarboxylate, form a sealed plug layer, improve retention time and shear dilution resistance, and enhance the matching degree and curing ability of leak plugging materials.
Under 8MPa conditions, the amount of HTHP water loss can reach 206.6mL, forming an efficient dense segment plug, extending the sealing time, enhancing the pressure and temperature resistance of the plug layer, reducing reservoir damage, and maintaining a good viscosity mold after aging Recovery volume and reduce drilling fluid releasing.
Smart Images

Figure CN118895111A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oilfield chemicals, and particularly relates to a pressure-bearing plugging material and drilling fluid for treating malignant leakage in fractured formations and applications thereof. Background Art
[0002] During the drilling process in fractured formations, drilling fluid leakage occurs frequently, in large amounts, and at high rates. Some formations with larger fractures and holes may even experience loss of return fluid, which greatly increases the cost of plugging a single well and may even cause the wellbore to be scrapped, resulting in significant economic losses.
[0003] At present, the plugging technologies at home and abroad, such as "one-bag" plugging technology, curable plugging technology, chemical cross-linking plugging technology, intelligent plugging technology, cementing and sealing technology, still have the following shortcomings: ① The leakage channels such as natural fractures, secondary fractures and induced fractures in the formation are affected by the exciting pressure (or increasing the density of drilling fluid), and there are expansion and closing phenomena. The drilling fluid has poor pressure bearing capacity, the retention time of plugging materials is short, and the frequency of drilling fluid leakage is high; ② The plugging material has a poor matching degree with the fracture size and is not easy to enter the leaking layer. At the same time, the particles themselves have insufficient pressure resistance and small friction resistance between particles. The formed plugging layer is easy to be destroyed under high temperature and high pressure, and spitting phenomenon occurs; ③ The plugging material is easily sheared, dispersed and thinned during the long-term circulation process, which increases the thixotropic properties of the drilling fluid and produces a large pressure excitation; ④ The plugging layer formed in the fracture has poor acid solubility and oil solubility, and it is not easy to unblock it in the later stage, causing irreversible reservoir damage. Summary of the invention
[0004] In view of the above problems, the present invention provides a pressure-bearing plugging material, drilling fluid and application for malignant leakage in fractured formations. The pressure-bearing plugging material has a high degree of matching with the fracture size, is easy to enter the leaking layer, has a long retention time, has good compatibility with the drilling fluid and is resistant to shear dilution. The plugging layer formed has a dense structure, strong pressure and high temperature bearing capacity, is easy to unblock, and has little damage to the reservoir. It can be used to prepare an excellent pressure-bearing plugging working fluid to ensure safe and efficient drilling of fractured formations, shorten the drilling cycle, and reduce the cost of completing a single well.
[0005] The first aspect of the present invention provides a pressure-bearing plugging material for severe leakage in fractured formations, which comprises the following raw material components, measured in parts by weight: 20-25 parts by weight of a plugging agent, 2-6 parts by weight of a filling binder, 1-2 parts by weight of an active agent, and 1-2 parts by weight of a dispersant; preferably, it comprises the following raw material components: 20 parts by weight of a plugging agent, 4 parts by weight of a filling binder, 1 part by weight of an active agent, and 1 part by weight of a dispersant.
[0006] The plugging agent is selected from at least one of diatomaceous earth, ultrafine calcium carbonate, mica flakes, walnut shell powder, bamboo fiber and composite mineral fiber SQD-98; the filling binder is selected from at least one of white asphalt, asbestos fiber and sodium silicate; the active agent is selected from at least one of heavy calcium carbonate and silica fume; the dispersant is selected from at least one of humate, polycarboxylate and polyanionic cellulose.
[0007] The plugging material of the present invention is designed for the malignant leakage characteristics of fractured formations, wherein the plugging agent forms a plugging skeleton in the fracture, and the filling binder fills the internal space of the plugging agent particles and the gaps between the particles, thereby playing a role in tightly sealing the leakage channel. The filling material active agent plays an orientation and stacking role, which can enhance the matching degree between the particle size and shape of the plugging material and the leakage channel, form a dense segment plug, and improve the retention and solidification ability of the plugging material. The dispersant plays a role in improving the rheology and sedimentation stability of the drilling fluid system in the wellbore.
[0008] The plugging agent is composed of diatomite, ultrafine calcium carbonate and mica flakes; preferably, the mass ratio of the diatomite, ultrafine calcium carbonate and mica flakes is 1-2:1-2:1-2; more preferably, the mass ratio of the diatomite, ultrafine calcium carbonate and mica flakes is 2:1:1. Diatomite, ultrafine calcium carbonate and mica flakes form a high water loss composite plugging agent, which forms a plugging skeleton in the cracks and uses the "filtering aid" effect of diatomite to make it lose water rapidly under the pressure difference generated by the drilling fluid column pressure and the formation pressure, thereby playing a better role in plugging the leakage channel.
[0009] The average particle size of the diatomaceous earth is 30-40 μm, the average particle size of the ultrafine calcium carbonate is 13-30 μm, and the diameter of the mica flakes is 840-2000 μm.
[0010] The filling binder is composed of white asphalt, asbestos fiber and sodium silicate; preferably, the mass ratio of the white asphalt, asbestos fiber and sodium silicate is 1-4:1-4:1-4; more preferably, the mass ratio of the white asphalt, asbestos fiber and sodium silicate is 1:2:1. The composite filling binder composed of white asphalt, asbestos fiber and sodium silicate can well fill the internal space of diatomaceous earth particles and the gaps between particles, thereby playing a role in better sealing and plugging the leakage channel.
[0011] The active agent is composed of heavy calcium carbonate and silica fume; preferably, the mass ratio of the heavy calcium carbonate to the silica fume is 0.5-1:0.5-1; more preferably, the mass ratio of the heavy calcium carbonate to the silica fume is 1:1; preferably, the mesh number of the heavy calcium carbonate is 300 mesh, and the mesh number of the silica fume is 300 mesh. The heavy calcium carbonate and silica fume form an acid-soluble composite active agent, which has the effect of better enhancing the matching degree between the particle size and shape of the plugging material and the leakage channel, forming a dense segment plug, and improving the retention and solidification capacity of the plugging material.
[0012] The dispersant is composed of humate and polycarboxylate; preferably, the mass ratio of humate to polycarboxylate is 0.5-1:0.5-1; more preferably, the mass ratio of humate to polycarboxylate is 1:1. The composite dispersant composed of humate and polycarboxylate has the effect of better improving the rheology and sedimentation stability of the drilling fluid system in the wellbore.
[0013] The second aspect of the present invention provides a drilling fluid, which is composed of the aforementioned pressure-bearing plugging material for vicious leakage in fractured formations and a base slurry; the base slurry can be conventionally selected from clean water, mud, and common water-based drilling fluid. Preferably, the added amount of the pressure-bearing plugging material for vicious leakage in fractured formations is 19-26% of the total weight of the drilling fluid.
[0014] The third aspect of the present invention provides a method for preparing the aforementioned drilling fluid: separately taking a plugging agent, a filling binder, an activator, a dispersant and a base slurry, stirring and mixing them evenly, the preparation is obtained.
[0015] A fourth aspect of the present invention provides the use of the pressure-bearing plugging material or drilling fluid for severe leakage in fractured formations in plugging fractured leakage formations.
[0016] The beneficial effects of the present invention are:
[0017] The invention prepares the pressure-bearing plugging material by compounding a plugging agent, a filling binder, an active agent and a dispersant composed of specific raw materials and supplementing them with a suitable weight ratio: 1) under the pressure of 8MPa, the HTHP (150°C) water loss can reach 206.6mL within 2min, and a dense segment plug can be quickly formed in the leakage channel to temporarily block the leakage channel, which can effectively increase the retention time of the plugging material, thereby preventing the fluid in the wellbore from flowing to the leakage formation gap; 2) the formed particle size gradation has a high matching degree with the development of the cracks, and the particle size of the drilling fluid system is mainly in the range of 0 to 4537μm (D50=394μm, D90=2010μm m), the particle size composition distribution has a multi-peak structure, the upper limit of the width of the plugged crack reaches 4.0mm, the pressure bearing capacity of the plugging layer can reach 8MPa, and the upper limit of temperature resistance can reach 150℃; 3) The formula has good compatibility. Before and after aging, and after repeated shearing at high and low rates, its viscosity modulus can still be restored, indicating that the pressure-bearing plugging material has excellent shear dilution resistance; in addition, after the pressure-bearing plugging material is added, the apparent viscosity of the drilling fluid before and after aging changes little, and the compatibility is good; 4) The acid solubility of the plugging layer formed by this formula is 85.8%, and after being dissolved in 150℃ white oil, the total solubility rate rises to 98.7%, that is, the residue is less than 2.0%, which can effectively reduce the damage to the reservoir. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a particle size distribution test diagram of the drilling fluid of the present invention;
[0019] Figure 2a The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 0.2 mm;
[0020] Figure 2b The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 0.5 mm;
[0021] Figure 2c The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 1.0 mm;
[0022] Figure 2d The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 2.0 mm;
[0023] Figure 2e The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 3.0 mm;
[0024] Figure 2f The HTHP plugging test results of the drilling fluid of the present invention at a seam width of 4.0 mm;
[0025] Figure 3 This is a curve diagram of the elastic modulus change of the drilling fluid of the present invention under alternating strain. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In the following examples, all raw materials were purchased from the market, and the raw material parameters are as follows:
[0028] Diatomaceous earth, appearance: white solid powder; average particle size: 30-40μm; specific surface area: ≤1000m 2 / g; loose density: ≤3.12g / cm 3 ; Suspension: 97-99%;
[0029] Ultrafine calcium carbonate, appearance: white solid powder; composed of 425 mesh ultrafine calcium carbonate and 1000 mesh ultrafine calcium carbonate mixed in a mass ratio of 1:2; particle size: 13-30μm;
[0030] Mica flakes, appearance: gray solid material; morphology: pseudo-hexagonal plate-like, short columnar; diameter: 840-2000μm; loose density: ≤3.44g / cm 3 ; Mineral density: 2.7-2.85g / cm3;
[0031] White asphalt, appearance: white or slightly yellow granules or powder; pH value: 7-10; water-soluble matter content: ≥40%; oil-soluble matter content: ≥40%; fluorescence level: ≤5;
[0032] Asbestos fiber, appearance: white; mesh: 100 mesh; particle size: 1-3mm; hardness: 2-2.5; mass: 600g / cm;
[0033] Sodium silicate, Appearance: Colorless or translucent liquid; Relative density: 2.614g / cm 3 ;Solubility: soluble in water;
[0034] Silica fume powder: Appearance: gray powder; Density: 2.78-2.91; pH value: 6; Thermal expansion coefficient: 6.5-10.6; Mohs hardness: 5.0; Mesh size: 300 mesh;
[0035] Heavy calcium carbonate: Appearance: white solid powder; Mesh size: 300 mesh; Bulk density: 1.7g / cm 3 ; Apparent density is 1.8g / cm 3 ;
[0036] Sodium humate: Appearance: bright color; Density: 1.4g / cm 3 ;Mesh number: 80-120 mesh;
[0037] Sodium polycarboxylate: Appearance: colorless transparent liquid; Viscosity: 350-500MPa·s; pH value: 7-8; Active ingredient: 40%;
[0038] In the following examples, the plugging agent is composed of diatomaceous earth, ultrafine calcium carbonate and mica flakes in a mass ratio of 2:1:1; the filling binder is composed of white asphalt, asbestos fiber and sodium silicate in a mass ratio of 1:2:1; the activator is composed of heavy calcium carbonate and silica fume in a mass ratio of 1:1; the dispersant is composed of sodium humate and sodium polycarboxylate in a mass ratio of 1:1; and the base slurry is taken from the on-site water-based drilling fluid.
[0039] Example 1
[0040] A drilling fluid, the formula and preparation method are as follows:
[0041] Formula: 20 parts by weight of plugging agent, 2 parts by weight of filling binder, 1.5 parts by weight of active agent, 1 part by weight of dispersant, and 100 parts by weight of base slurry;
[0042] Preparation method: Step 1: Take the base slurry into a high-stirring cup, turn on the agitator, adjust the speed to 4000r / min for stirring; Step 2: Add the plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add the filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add the active agent to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add the dispersant to the high-stirring cup, adjust the speed to 6000r / min, and stir for 30 minutes.
[0043] Example 2
[0044] A drilling fluid, the formula and preparation method are as follows:
[0045] Formula: 22.5 parts by weight of plugging agent, 4 parts by weight of filling binder, 1 part by weight of active agent, 1 part by weight of dispersant, and 100 parts by weight of clean water;
[0046] Preparation method: Step 1: Pour clean water into a high-stirring cup, turn on the agitator, adjust the speed to 6000r / min for stirring; Step 2: Add a plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add a filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add an active agent to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add a dispersant to the high-stirring cup, adjust the speed to 8000r / min, and stir for 30 minutes.
[0047] Example 3
[0048] A drilling fluid, the formula and preparation method are as follows:
[0049] Formula: 25 parts by weight of plugging agent, 4 parts by weight of filling binder, 2 parts by weight of active agent, 1 part by weight of dispersant, and 100 parts by weight of base slurry;
[0050] Preparation method: Step 1: Take the base slurry into a high-stirring cup, turn on the agitator, adjust the speed to 5000r / min for stirring; Step 2: Add the plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add the filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add the activator to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add the dispersant to the high-stirring cup, adjust the speed to 7000r / min, and stir for 30 minutes.
[0051] Example 4
[0052] A drilling fluid, the formula and preparation method are as follows:
[0053] Formula: 20 parts by weight of plugging agent, 5 parts by weight of filling binder, 1 part by weight of active agent, 2 parts by weight of dispersant, 100 parts by weight of base slurry;
[0054] Preparation method: Step 1: Take the base slurry into a high-stirring cup, turn on the agitator, adjust the speed to 5000r / min for stirring; Step 2: Add the plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add the filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add the activator to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add the dispersant to the high-stirring cup, adjust the speed to 7000r / min, and stir for 30 minutes.
[0055] Example 5
[0056] A drilling fluid, the formula and preparation method are as follows:
[0057] Formula: 25 parts by weight of plugging agent, 6 parts by weight of filling binder, 2 parts by weight of active agent, 2 parts by weight of dispersant, 100 parts by weight of base slurry;
[0058] Preparation method: Step 1: Take the base slurry into a high-stirring cup, turn on the agitator, adjust the speed to 5000r / min for stirring; Step 2: Add the plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add the filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add the activator to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add the dispersant to the high-stirring cup, adjust the speed to 7000r / min, and stir for 30 minutes.
[0059] Example 6
[0060] A drilling fluid, the formula and preparation method are as follows:
[0061] Formula: 20 parts by weight of plugging agent, 4 parts by weight of filling binder, 1 part by weight of active agent, 1 part by weight of dispersant, 100 parts by weight of base slurry;
[0062] Preparation method: Step 1: Take the base slurry into a high-stirring cup, turn on the agitator, adjust the speed to 5000r / min for stirring; Step 2: Add the plugging agent to the high-stirring cup, and continue stirring for 15 minutes; Step 3: Add the filling binder to the high-stirring cup, and continue stirring for 15 minutes; Step 4: Add the activator to the high-stirring cup, and continue stirring for 20 minutes; Step 5: Add the dispersant to the high-stirring cup, adjust the speed to 7000r / min, and stir for 30 minutes.
[0063] Test example
[0064] 1. Formula screening test study
[0065] 1. Screening of plugging agents:
[0066] Taking the cumulative leakage of 4.0 mm seam plate at 6 MPa pressure as the evaluation index, the seven-factor two-level orthogonal table L8 (27) was selected to add a combination of plugging materials to the on-site drilling fluid to evaluate its plugging capacity. See Tables 1 and 2.
[0067] Among them, the plugging performance of the 4mm seam plate under 6MPa pressure is evaluated by the DL plugging material evaluation device to evaluate the plugging performance of the plugging material used. The specific steps are as follows:
[0068] ①Prepare the plugging slurry, heat it at 150℃ for 16 hours, and stir it on an electric mixer for 30 minutes;
[0069] ②Pour the slurry into the DL plugging instrument and install the gas source manifold;
[0070] ③ Increase the pressure at a rate of 0.069 MPa per second to the target pressure, or until the plug is destroyed and the drilling fluid in the instrument container flows out, record the volume of drilling fluid flowing out and the maximum pressure reached. If the plug is successful, maintain the pressure for 10 minutes and record the final drilling fluid volume.
[0071] Acid solubility test of plugging materials:
[0072] The acid solubility test of the plugging material is used to evaluate the acid solubility of the plugging material. The main experimental instruments are a mixer and a drying oven. The experiment is carried out with reference to the petroleum industry standard SYT / 5061-93 "Limestone powder for drilling fluid". The specific steps are as follows:
[0073] ① Weigh 2 g (accurate to 0.01 g) of the sample dried at 105±3℃ for 2 h, put it into a 200 mL beaker, add 30 mL of 15% mixed acid solution (mainly composed of hydrochloric acid and hydrofluoric acid) in succession, cover it, and after the reaction stops, transfer it to a Buchner funnel for suction filtration, and wash with distilled water until there is no chloride ion (check with 1% (m / m) silver nitrate solution).
[0074] ② Place the Buchner funnel in a drying oven at 150±3℃ and dry it for 2 hours. Take it out and place it in a desiccator. After cooling to room temperature, weigh it.
[0075] Calculation: Acid insoluble matter = (m3 – m2) / m1 × 100%
[0076] Where: m3——mass of filter paper and residue, g;
[0077] m2——filter paper mass, g;
[0078] m1——sample mass, g.
[0079] Table 1 Orthogonal experimental design table
[0080]
[0081] Table 2 Orthogonal experiment results
[0082]
[0083] Through range (Rj) analysis, comprehensive consideration of the impact on leakage and plugging resistance (acid solubility), diatomaceous earth, ultrafine calcium carbonate and flaky mica were selected to form the formula of high water loss composite plugging agent, and the addition ratio was 2:1:1.
[0084] Taking the cumulative leakage at 6MPa pressure of 4.0mm seam plate as the inspection index, 22.5% of the plugging material combination (diatomite: ultrafine calcium carbonate: flaky mica flakes = 2:1:1) was added to the on-site drilling fluid to evaluate its plugging capacity. See Table 3.
[0085] Table 3 Performance evaluation test results
[0086]
[0087] It was determined that diatomaceous earth, ultrafine calcium carbonate and flaky mica flakes were selected to form the formula of high water loss composite plugging agent, and the addition ratio was 2:1:1.
[0088] 2. Screening of filling binders, see Table 4.
[0089] Table 4 Results of the filling binder screening test
[0090]
[0091] Base slurry: On-site drilling fluid + 20.0% plugging agent (diatomaceous earth: ultrafine calcium carbonate: flaky mica flakes = 2:1:1)
[0092] The optimal ratio of filling binder white asphalt particles, asbestos fibers and sodium silicate was determined to be 1:2:1. Under 6MPa conditions, the filtration loss of 4.0mm seam plate was reduced to 208.2mL.
[0093] 3. Screening of active agents, see Table 5.
[0094] Table 5 Results of the active agent screening test
[0095]
[0096] Base slurry: On-site drilling fluid + 20.0% plugging agent (diatomaceous earth: ultrafine calcium carbonate: flaky mica = 2:1:1) + 4.0% filling binder (white asphalt particles: asbestos fiber: sodium silicate = 1:2:1)
[0097] It was determined that the optimal composition of the active agent was silica fume powder and heavy calcium carbonate in a 1:1 ratio. Under 8MPa conditions, the filtration loss of the 4.0mm seam plate was reduced to 238.8mL, which can further improve the pressure-bearing capacity of the plugging slurry.
[0098] 4. Dispersant screening, see Table 6.
[0099] Table 6 Dispersant screening test results
[0100]
[0101] Base slurry: on-site drilling fluid + 20.0% plugging agent (diatomaceous earth: ultrafine calcium carbonate: flaky mica = 2:1:1) + 4.0% filling binder (white asphalt particles: asbestos fiber: sodium silicate = 1:2:1) + 1.0% activator (silica ash powder: heavy calcium carbonate = 1:1); aging conditions: 150℃×16h.
[0102] After adding 0.5% sodium humate + 0.5% sodium polycarboxylate to the base slurry, the apparent viscosity and plastic viscosity of the base slurry decreased by 3-5 mPa·s, the dynamic shear force remained stable, but the dynamic-plastic ratio increased significantly, indicating that the rock-carrying performance of the drilling fluid was enhanced. In addition, under 8MPa conditions, the filtration loss of the 4.0mm seam plate was further reduced to 234.8mL, and the plugging ability was stronger.
[0103] 2. Performance Test
[0104] 1. Particle size distribution test
[0105] Referring to the determination standard of particle size distribution in 3.3.2 of the petroleum industry "Indoor test method for bridging plugging materials for drilling fluids SY / T 5840-2007", the particle size distribution of the drilling fluid prepared in Example 6 was determined. The experimental results are as follows: Figure 1 The particle size of the drilling fluid prepared by the present invention is mainly in the range of 0 to 4537 μm (D50=394 μm, D90=2010 μm), and the particle size composition distribution has a multi-peak structure, which is conducive to plugging cracks of different sizes and improving the plugging effect.
[0106] 2. Evaluation of plugging performance
[0107] The plugging performance of the drilling fluid prepared in Example 6 was evaluated by a high temperature and high pressure plugging tester. The specific steps are as follows: ① Prepare the drilling fluid and stir it on an electric stirrer for 30 minutes; ② Select crack type templates of different widths (0.2mm, 0.5mm, 1.0mm, 2.0mm, 3.0mm and 4.0mm), put the template into the test cup, and assemble it into a test assembly; ③ Inject 2000mL of drilling fluid into the test container; ④ Pre-apply 2.0MPa pressure to the test container and set the temperature to 150℃; ⑤ Uniformly pressurize, each time 0.5-1.0MPa, and each pressure point after pressurization needs to be stabilized for 10 minutes before starting the timer and recording the leakage; ⑥ Pressurize to 8.0MPa and stabilize for 60 minutes.
[0108] The experimental results are shown in Figure 2. The drilling fluid of the present invention matches a wide width of crack plugging, can bear pressure to plug cracks with a width of 0.2mm to 4.0mm, the upper limit of the pressure bearing capacity of the plugging layer can reach 8MPa, the temperature resistance of the plugging material is greater than 150°C, and the overall performance is good; among them, for a 4.00mm seam plate under a pressure of 8MPa, the HTHP water loss within 2min can reach 206.6mL, indicating that the drilling fluid can quickly lose water at the leakage channel to form a dense segment plug, which can effectively solve the malignant leakage of fractured formations and ensure safe and efficient drilling of formations prone to leakage.
[0109] 3. Evaluation of acid and oil solubility
[0110] With reference to the petroleum industry standard SYT / 5061-93 "Limestone powder for drilling fluid", the acid solubility and oil solubility evaluation experiments were conducted on the drilling fluid of Example 6. The test results are shown in Table 7. The acid solubility effect is very good, and the acid solubility rate in 15% hydrochloric acid can reach more than 85%. After being dissolved in 150°C white oil, the solubility rate rises to 98.2%, that is, the residue is less than 2.0%, indicating that it is easy to remove blockage in the later stage and can effectively reduce the damage to the reservoir.
[0111] Table 7 Acid and oil soluble test results of plugging materials
[0112]
[0113] 4. Rheological properties evaluation
[0114] With reference to the national standard GB / T 16783.1-2014 "Field Test of Drilling Fluids in the Petroleum and Natural Gas Industry Part 1: Water-Based Drilling Fluids", the rheological properties of the drilling fluid in Example 6 were evaluated. The test results are shown in Table 8. The plugging material has little effect on the viscosity and filtration of the drilling fluid, the apparent viscosity increases slightly, and the filtration loss remains basically stable.
[0115] Table 8 Rheological properties evaluation
[0116]
[0117]
[0118] Aging conditions: 150℃×16h. High temperature and high pressure filtration test: 150℃×3.5MPa, 30min.
[0119] 5. Lubrication performance evaluation
[0120] With reference to the petroleum industry specification SY / T6094-94 "Evaluation Procedure for Lubricants for Drilling Fluids", the lubrication performance of the drilling fluid of Example 6 was tested using an extreme pressure lubrication instrument. The test results are shown in Table 9. The pressure-bearing plugging material of the present invention has little effect on the lubricity of the base slurry and has strong compatibility.
[0121] Table 9 Lubrication performance evaluation
[0122]
[0123] 6. Evaluation of shear thinning resistance
[0124] According to the HAKKE rheometer test steps, the change of its viscous modulus under the action of alternating strain is measured. The test results are as follows Figure 3 It can be seen that the viscosity modulus of the drilling fluid in Example 6 can still be restored after repeated shearing at high and low rates before and after aging, indicating that the drilling fluid has excellent anti-shear dilution performance, which can ensure the pumpability and retention and plugging ability during the on-site construction process, and reduce the drilling fluid leakage phenomenon in the later drilling process.
[0125] The present invention also carried out the above-mentioned performance tests on the remaining embodiments, and the test results were substantially the same, which will not be described in detail due to space limitations.
[0126] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
Claims
1. A pressure-bearing plugging material for treating malignant leakage in fractured formations, characterized in that: By weight, it includes the following raw material components: 20-25 parts by weight of plugging agent, 2-6 parts by weight of filling binder, 1-2 parts by weight of active agent, and 1-2 parts by weight of dispersant; The plugging agent is selected from at least one of diatomaceous earth, ultrafine calcium carbonate, mica flakes, walnut shell powder, bamboo fiber and composite mineral fiber SQD-98; The filling binder is selected from at least one of white asphalt, asbestos fiber and sodium silicate; The active agent is selected from at least one of heavy calcium carbonate and silica fume; The dispersant is selected from at least one of humate, polycarboxylate and polyanionic cellulose.
2. The pressure-bearing plugging material for treating malignant leakage in fractured formations according to claim 1, characterized in that: By weight, it includes the following raw material components: 20 parts by weight of plugging agent, 4 parts by weight of filling binder, 1 part by weight of activator and 1 part by weight of dispersant.
3. The pressure-bearing plugging material for treating malignant leakage in fractured formations according to claim 1, characterized in that: The plugging agent is composed of diatomite, ultrafine calcium carbonate and mica flakes; Preferably, the mass ratio of the diatomaceous earth, ultrafine calcium carbonate and mica flakes is 1-2:1-2:1-2; More preferably, the mass ratio of the diatomaceous earth, ultrafine calcium carbonate and mica flakes is 2:1:
1.
4. The pressure-bearing plugging material for malignant leakage in fractured formations according to any one of claims 1 to 3, characterized in that: The average particle size of the diatomaceous earth is 30-40 μm, the average particle size of the ultrafine calcium carbonate is 13-30 μm, and the diameter of the mica flakes is 840-2000 μm.
5. The pressure-bearing plugging material for treating malignant leakage in fractured formations according to claim 1, characterized in that: The filling binder is composed of white asphalt, asbestos fiber and sodium silicate; Preferably, the mass ratio of the white asphalt, asbestos fiber and sodium silicate is 1-4:1-4:1-4; More preferably, the mass ratio of the white asphalt, asbestos fiber and sodium silicate is 1:2:
1.
6. The pressure-bearing plugging material for treating malignant leakage in fractured formations according to claim 1, characterized in that: The active agent consists of heavy calcium carbonate and silica fume powder; Preferably, the mass ratio of the heavy calcium carbonate to the silica fume powder is 0.5-1:0.5-1; more preferably, the mass ratio of the heavy calcium carbonate to the silica fume powder is 1:1; Preferably, the mesh size of the heavy calcium carbonate is 300 mesh, and the mesh size of the silica fume powder is 300 mesh.
7. The pressure-bearing plugging material for treating malignant leakage in fractured formations according to claim 1, characterized in that: The dispersant is composed of humate and polycarboxylate; Preferably, the mass ratio of humate to polycarboxylate is 0.5-1:0.5-1; More preferably, the mass ratio of the humate to the polycarboxylate is 1:
1.
8. A drilling fluid, characterized in that: The method comprises the pressure-bearing plugging material for vicious leakage in fractured formations as claimed in any one of claims 1 to 7 and base slurry; preferably, the added amount of the pressure-bearing plugging material for vicious leakage in fractured formations is 19-26% of the total weight of the drilling fluid.
9. A method for preparing the drilling fluid according to claim 8, characterized in that: The preparation method comprises the following steps: respectively taking a plugging agent, a filling binder, an active agent, a dispersant and a base slurry, stirring and mixing them evenly to obtain the product.
10. Use of the pressure-bearing plugging material for severe leakage in fractured formations as claimed in any one of claims 1 to 7 or the drilling fluid as claimed in claim 8 in plugging fractured leakage formations.
Citation Information
Patent Citations
High-water-loss curing plugging agent for plugging fissures
CN102977866A
Crack plugging agent for oil-base drilling fluids
CN104232037A
Composite material plugging agent for water plugging and leaking plugging of horizontal well and preparation method of composite material plugging agent
CN113480254A
Fast-water-loss plunger type plugging agent for drilling fluid and preparation method of plugging agent
CN114045160A
A fiber suspending agent for lost-circulation materials
US20160257869A1
Cited By
Water-based drilling fluid high-temperature-resistant plugging agent as well as preparation method and device thereof
CN121064812A
Water-based high-temperature-resistant leak sealing agent for drilling fluid, and preparation method and device thereof
CN121064812B