Welding method for eliminating residual stress defect of surfacing layer of steel casting

By employing multi-layer tempering weld technology and flaw detection methods, the problem of residual stress defects during the welding process of large cast steel structural components for suspension bridges was solved, achieving efficient, economical, and controllable welding repair results and improving the durability and quality of the structure.

CN118951244APending Publication Date: 2024-11-15DEYANG TIANYUAN HEAVY IND
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411300601.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively eliminate residual stress defects generated during the welding process of large cast steel structural components for suspension bridges, such as cable clamps, cable saddles, and cable sleeves, leading to structural cracking and durability issues. Furthermore, existing stress relief methods are inefficient and have uncontrollable quality.

Method used

Multi-layer tempering welding technology is adopted, which forms multiple weld beads through gas shielded welding. Thermal cycling and grinding are carried out between each weld bead, and ultrasonic and magnetic particle testing are combined to ensure welding quality.

Benefits of technology

It effectively eliminates residual stress defects in large cast steel structural components, improves manufacturing efficiency and finished product quality, reduces cracking risk, and achieves efficient, economical, and controllable welding repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047543090000101
    Figure BDA0005047543090000101
  • Figure BDA0005047543090000102
    Figure BDA0005047543090000102
  • Figure BDA0005047543090000111
    Figure BDA0005047543090000111
Patent Text Reader

Abstract

The invention discloses a welding method for eliminating residual stress defects of a surfacing layer of a steel casting. The welding method comprises the following steps: 1, pretreating a welding groove on a workpiece; 2, preheating the welding groove to 150 to 200 DEG C; 3, welding a welding bead of a base layer on the welding groove in a gas shield welding manner; 4, polishing a weld bead of the base layer to remove 1 / 3-2 / 3 of the thickness of the weld bead; 5, filling a first layer of welding bead on the ground base layer welding bead in a gas shield welding manner; the step 4 and the step 5 are repeated until the welding groove is filled with surfacing welding; 6, the topmost layer filled with surfacing welding is polished to remove 1 / 3-2 / 3 of the thickness of the topmost layer; 7, welding a cover layer welding bead at the topmost layer of the filling surfacing welding in a gas shield welding manner, wherein the edge of the cover layer welding bead is in clearance fit with the base metal; and 8, removing redundant surfacing structures on the welding grooves, and performing flaw detection. By means of the tempering bead welding technology, welding repair is naturally formed in the welding process of the filling surfacing layer, and the method has the technical characteristics of being easy, economical, efficient, controllable in quality and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a welding process for steel castings, in particular to a welding method for eliminating residual stress defects in a cladding layer of a steel casting. Background Art

[0002] In the suspension bridge structure, the main cable saddles, loose cable saddles, cable clamps and loose cable sleeves, which are the core force-bearing structural parts, are usually made of cast steel. They are subjected to huge structural stress in the working environment. Therefore, the technical requirements for product quality are as high as possible during manufacturing.

[0003] Structural parts such as saddles, cable clamps, loose cable sleeves, etc. made of steel castings need to be welded through multiple welds due to their complex molding structures. In addition, due to the material properties of the steel castings themselves, local repair welding is required. It is well known in the industry that at each weld (i.e., welding part), compression yielding occurs around the melting area when the material is heated and expanded during welding, and the material shrinks when the metal cools, causing residual stress in the structure. If the residual stress in the product structure is not released accordingly, plastic deformation will occur over time, and then the superposition of stress during use will easily lead to structural cracking, which directly affects the force and durability. Therefore, for structural parts such as saddles, cable clamps, loose cable sleeves, etc. made of steel castings, each weld should be subjected to post-weld stress relief treatment as much as possible.

[0004] At present, the stress relief treatment of the welded parts or repaired welded parts of steel castings is mainly achieved through three methods: natural aging stress relief, heat treatment stress relief, and vibration stress relief. Natural aging stress relief has the defects of being too long and uncontrollable. Both heat treatment stress relief and vibration stress relief have high technical requirements for equipment. Since the cable saddles, cable clamps, loose cable sleeves and other structural parts used in suspension bridges are large-scale cast steel structures, there are currently no suitable heat treatment stress relief equipment and vibration stress relief equipment available. Therefore, the cable saddles, cable clamps, loose cable sleeves and other structural parts used in suspension bridges usually adopt the natural aging stress relief method after welding, which not only has the technical problems of long manufacturing cycle and low manufacturing efficiency, but also poor quality controllability.

[0005] In the early 1980s, the industry developed a welding repair technology that can replace post-weld heat treatment, namely tempering weld technology. Tempering weld technology is a welding technology that improves the structure and performance of the stacked welds through the thermal cycle of subsequent welds. In the currently disclosed technology of eliminating residual stress defects in the weld overlay of cast steel parts by tempering welds, only a capping weld is welded at the topmost layer of the filling weld overlay, and the heat generated by the excess capping weld affects the grains in the filling weld overlay, improves the microstructure and properties of the filling weld overlay, and finally removes the excess capping weld by grinding. For example, the Chinese patent document discloses a technology named "an on-site welding repair method particularly suitable for weld overlay defects on low alloy and carbon steel", with publication number CN 104084749A and publication date October 8, 2014, a technology named "a welding method for capping welds of submerged arc welding seams of high-strength low-alloy steel", with publication number CN 110935990 A and publication date March 31, 2020, and a technology named "an automatic tempering weld overlay method for pipeline maintenance", with publication number CN 107186317A and publication date September 22, 2017.

[0006] However, since the heat affected depth area generated by a single cover layer weld is too limited, it is difficult to form a sufficient thermal impact on the large-sized filling weld layer on large structural parts such as cable clamps, cable saddles, and loose cable sleeves. Therefore, it is only suitable for the heat dissipation of small-sized weld layers. Currently, there is no disclosed tempering weld technology that can be applied to large structural parts such as cable clamps, cable saddles, and loose cable sleeves.

[0007] If the tempering weld technology can be effectively applied to large cast steel structures such as cable clamps, cable saddles, and loose cable sleeves, welding repairs can be formed naturally during the welding process, with little need for additional stress relief treatment, thereby greatly improving manufacturing efficiency and finished product quality through controllable technical means. Summary of the invention

[0008] The technical purpose of the present invention is to provide a welding method based on tempering weld technology to eliminate residual stress defects in the weld overlay layer of cast steel parts in view of the particularity and high-quality technical requirements of the above-mentioned large cast steel structural parts such as cable clamps, cable saddles, and loose cable sleeves after welding, as well as the shortcomings of the existing technology.

[0009] The technical purpose of the present invention is achieved by the following technical solution: a welding method for eliminating residual stress defects in the weld overlay of a steel casting, the welding method comprising the following process steps:

[0010] Step 1. Pre-treat the welding groove on the workpiece;

[0011] Step 2. Preheat the welding groove area to 150-200°C;

[0012] Step 3. Weld the base weld on the welding groove by gas shielded welding;

[0013] Step 4. Grind away 1 / 3 to 2 / 3 of the thickness of the base weld from the top side;

[0014] Step 5. Using gas shielded welding, fill the first layer of welds on the ground base welds;

[0015] The process of using the adjacent previous weld bead as the grinding basis and the subsequent weld bead heat treating the previous weld bead is repeated in steps 4 and 5 until the welding groove is filled with surfacing;

[0016] Step 6. Grind away 1 / 3 to 2 / 3 of the thickness of the top layer of the filler cladding from the top side;

[0017] Step 7. Performing welding of the cap layer weld at the topmost layer of the filling cladding in step 6 by means of gas shielded welding, and forming a gap fit between the edge of the cap layer weld and the base material of the workpiece;

[0018] Step 8. Remove the excess weld structure on the weld groove and perform flaw detection.

[0019] Furthermore, the workpiece base material is a ZG20Mn steel casting, and the welding wire used is an ER50-6 welding wire with a diameter of 1.2 mm;

[0020] In step 3, the welding parameters of the base weld are: shielding gas CO2, shielding gas flow rate 20-25 L / min, current 240-300 A, voltage 26-32 V, current polarity direct and reverse, welding speed 35-45 cm / min;

[0021] In step 5, the welding parameters of the filling layer weld are: shielding gas CO2, shielding gas flow rate 20-25L / min, current 260-320A, voltage 28-36V, current polarity direct and reverse, welding speed 40-50cm / min;

[0022] In step 7, the welding parameters of the cover layer weld are: shielding gas CO2, shielding gas flow rate 20-25L / min, current 260-320A, voltage 28-36V, current polarity direct and reverse, and welding speed 40-50cm / min.

[0023] Furthermore, the workpiece is a cable clamp, a cable saddle or a loose cable sleeve for a suspension bridge.

[0024] Furthermore, in step 1, the pretreatment is to grind the welding groove on the workpiece to be smooth, and to detect and confirm that there are no defects before welding. Further, the detection method of the detection confirmation is penetration testing + magnetic particle testing.

[0025] Furthermore, the welding groove on the workpiece is a U-shaped groove.

[0026] Furthermore, the grinding is performed manually using an angle grinder.

[0027] Furthermore, in step 7, the fitting clearance between the edge of the cover layer weld and the workpiece base material is 2 to 3 mm.

[0028] Furthermore, in step 8, the flaw detection method is ultrasonic flaw detection + magnetic particle flaw detection;

[0029] The ultrasonic flaw detection result meets the Level 1 standard in GB / T7233.1-2023;

[0030] The results of the magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

[0031] The beneficial technical effect of the present invention is as follows: the above technical measures are aimed at the special characteristics and high-quality technical requirements of large cast steel structural parts such as cable clamps, cable saddles, loose cable sleeves, etc. for suspension bridges, which have residual stress defects after welding. The tempering weld bead technology is used to improve the structure and performance of the first layer of weld bead by the thermal cycle of the second layer of weld bead adjacent to the stack, so as to form a welding structure of multi-layer tempering weld bead, and the first layer of weld bead adjacent to the stack is almost half ground, so as to enhance the heat of the second layer of weld bead to fully affect the first layer of weld bead, ensure the tempering effect of the coarse grains of the first layer of weld bead, make the grains of the first layer of weld bead fine and dense, reduce the hardness of the weld and the heat-affected zone, and thus reduce the risk of cracking of the finished product. It can effectively adapt to the large-size (or large-depth) filling cladding layer of large cast steel structural parts including cable clamps, cable saddles, loose cable sleeves, so that welding repair is naturally formed during the welding process of the large-size filling cladding layer, and has the technical characteristics of being easy, economical, efficient, and quality-controlled. DETAILED DESCRIPTION

[0032] The present invention relates to a welding process for steel castings, and specifically to a welding method for eliminating residual stress defects in a weld overlay of a steel casting. The main technical solution of the present invention is specifically described below in conjunction with a plurality of embodiments. In addition, the expressions "approximately" and "substantially" regarding quantities or matching relationships in the following text mean that reasonable assembly errors, processing errors, etc. in the industry are allowed to exist, and do not literally express absolute quantities or matching relationships.

[0033] Example 1

[0034] The present invention uses ZG20Mn steel castings to manufacture cable clamps for suspension bridges. There are local repair welding parts on the cable clamp structure. The local repair welding parts need to be repaired by surfacing welding. Specifically, the following welding method is used to perform surfacing welding repair and eliminate residual stress defects in the surfacing welding parts, including the following process steps:

[0035] Step 1. The part to be repaired on the workpiece (i.e. the cable clamp structure, the same below) is machined to form a welding groove to form a relatively spacious and easy-to-operate U-shaped welding groove;

[0036] Use a grinding wheel to grind the welding groove on the workpiece to make it smooth, and use the method of penetration testing + magnetic particle flaw detection to test the welding groove on the workpiece to confirm that there are no defects before welding;

[0037] Step 2. Preheat the welding groove area on the workpiece to 180°C;

[0038] Step 3. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the base weld on the welding groove by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 23 L / min, current 280 A, voltage 28 V, current polarity straight reverse, and welding speed 40 cm / min;

[0039] Step 4. To ensure that the adjacent subsequent welds can form a sufficient and dense thermal impact on the base weld and achieve the tempering effect on the coarse grains, the base weld is manually ground from the top side using an angle grinder to remove about 1 / 2 of the thickness of the base weld by grinding;

[0040] Step 5. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the first layer of filler weld on the ground base weld by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 23 L / min, current 300 A, voltage 32 V, current polarity direct and reverse, and welding speed 45 cm / min;

[0041] According to the process that the adjacent previous weld is used as the grinding basis and the next weld is used to heat treat the previous weld, steps 4 and 5 are repeated, that is, after the first-layer filler weld is ground, the second-layer filler weld is welded on the ground first-layer filler weld; after the second-layer filler weld is ground, the third-layer filler weld is welded on the ground second-layer filler weld, and so on, until the welding groove is filled with surfacing;

[0042] Step 6. Use an angle grinder to manually grind the top layer of the filler weld from the top side to remove about 1 / 2 of the thickness of the top layer of the filler weld by grinding;

[0043] Step 7. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the cap layer weld on the top layer of the ground filler cladding by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow 23 L / min, current 300 A, voltage 32 V, current polarity direct and reverse, and welding speed 45 cm / min;

[0044] During the welding process of the cap weld, a clearance of about 3mm is required between the edge of the cap weld and the workpiece base material to avoid the formation of a new heat-affected zone between the cap weld and the workpiece base material to generate residual stress defects, that is, the heat-affected zone of the cap weld is only for the top layer of the filler cladding;

[0045] Step 8. Use an angle grinder to grind away the excess cladding structure on the welding groove to form a flat structure in the filled cladding area on the workpiece, and perform flaw detection on the filled cladding area of ​​the workpiece by ultrasonic flaw detection + magnetic particle flaw detection;

[0046] Among them, the results of ultrasonic flaw detection meet the Level 1 standard in GB / T7233.1-2023;

[0047] The results of magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

[0048] Example 2

[0049] The present invention uses ZG20Mn steel castings to manufacture a cable saddle for a suspension bridge. There are local repair welding parts on the cable saddle structural parts, and there are weld connection parts between the relative structural parts constituting the cable saddle. The aforementioned local repair welding parts and weld connection parts need to be formed by surfacing welding. Specifically, the following welding method is used to perform surfacing welding and eliminate residual stress defects in the surfacing welding parts, including the following process steps:

[0050] Step 1. The part to be repaired on the workpiece (i.e., the saddle structure, the same below) is machined to form a welding groove to form a relatively spacious and easy-to-operate U-shaped welding groove;

[0051] Use a grinding wheel to grind the welding groove on the workpiece to make it smooth, and use the method of penetration testing + magnetic particle flaw detection to test the welding groove on the workpiece to confirm that there are no defects before welding;

[0052] Step 2. Preheat the welding groove area on the workpiece to 150°C;

[0053] Step 3. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the base weld on the welding groove by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 20 L / min, current 240 A, voltage 26 V, current polarity direct and reverse, and welding speed 35 cm / min;

[0054] Step 4. To ensure that the adjacent subsequent welds can form a sufficient and dense thermal impact on the base weld and achieve the tempering effect on the coarse grains, the base weld is manually ground from the top side using an angle grinder to remove about 1 / 3 of the thickness of the base weld by grinding;

[0055] Step 5. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the first layer of filler weld on the ground base weld by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 20 L / min, current 260 A, voltage 28 V, current polarity direct and reverse, and welding speed 40 cm / min;

[0056] According to the process that the adjacent previous weld is used as the grinding basis and the next weld is used to heat treat the previous weld, steps 4 and 5 are repeated, that is, after the first-layer filler weld is ground, the second-layer filler weld is welded on the ground first-layer filler weld; after the second-layer filler weld is ground, the third-layer filler weld is welded on the ground second-layer filler weld, and so on, until the welding groove is filled with surfacing;

[0057] Step 6. Use an angle grinder to manually grind the top layer of the filler weld from the top side, removing about 1 / 3 of the thickness of the top layer of the filler weld by grinding;

[0058] Step 7. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the cap layer weld on the top layer of the ground filler cladding by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 20 L / min, current 260 A, voltage 28 V, current polarity direct and reverse, and welding speed 40 cm / min;

[0059] During the welding process of the cap weld, a clearance of about 2 mm is required between the edge of the cap weld and the workpiece base material to avoid the formation of a new heat-affected zone between the cap weld and the workpiece base material to generate residual stress defects, that is, the heat-affected zone of the cap weld is only for the top layer of the filler cladding;

[0060] Step 8. Use an angle grinder to grind away the excess cladding structure on the welding groove to form a flat structure in the filled cladding area on the workpiece, and perform flaw detection on the filled cladding area of ​​the workpiece by ultrasonic flaw detection + magnetic particle flaw detection;

[0061] Among them, the results of ultrasonic flaw detection meet the Level 1 standard in GB / T7233.1-2023;

[0062] The results of magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

[0063] Example 3

[0064] The present invention uses ZG20Mn steel castings to manufacture a loose cable sleeve for a suspension bridge. There are local repair welding parts on the loose cable sleeve, and there are weld connection parts between the relative structural parts constituting the loose cable sleeve. The aforementioned weld connection parts need to be formed by surfacing welding. Specifically, the following welding method is used to perform surfacing welding and eliminate residual stress defects at the surfacing welding parts, including the following process steps:

[0065] Step 1. The part to be repaired on the workpiece (i.e., the loose cable sleeve structural part, the same below) is machined to form a welding groove to form a relatively spacious and easy-to-operate U-shaped welding groove;

[0066] Use a grinding wheel to grind the welding groove on the workpiece to make it smooth, and use the method of penetration testing + magnetic particle flaw detection to test the welding groove on the workpiece to confirm that there are no defects before welding;

[0067] Step 2. Preheat the welding groove area on the workpiece to 200°C;

[0068] Step 3. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the base weld on the welding groove by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 25 L / min, current 300 A, voltage 32 V, current polarity straight reverse, welding speed 45 cm / min;

[0069] Step 4. To ensure that the adjacent subsequent welds can form a sufficient and dense thermal impact on the base weld and achieve the tempering effect on the coarse grains, the base weld is manually ground from the top side using an angle grinder to remove about 2 / 3 of the thickness of the base weld by grinding;

[0070] Step 5. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the first layer of filler weld on the ground base weld by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 25 L / min, current 320 A, voltage 36 V, current polarity direct and reverse, and welding speed 50 cm / min;

[0071] According to the process that the adjacent previous weld is used as the grinding basis and the next weld is used to heat treat the previous weld, steps 4 and 5 are repeated, that is, after the first-layer filler weld is ground, the second-layer filler weld is welded on the ground first-layer filler weld; after the second-layer filler weld is ground, the third-layer filler weld is welded on the ground second-layer filler weld, and so on, until the welding groove is filled with surfacing;

[0072] Step 6. Use an angle grinder to manually grind the top layer of the filler weld from the top side to remove about 2 / 3 of the thickness of the top layer of the filler weld by grinding;

[0073] Step 7. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the cap layer weld on the top layer of the ground filler cladding by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 25 L / min, current 320 A, voltage 36 V, current polarity direct and reverse, and welding speed 50 cm / min;

[0074] During the welding process of the cap weld, a clearance of about 2.5 mm is required between the edge of the cap weld and the workpiece base material to avoid the formation of a new heat-affected zone between the cap weld and the workpiece base material to generate residual stress defects, that is, the heat-affected zone of the cap weld is only for the top layer of the filler weld.

[0075] Step 8. Use an angle grinder to grind away the excess cladding structure on the welding groove to form a flat structure in the filled cladding area on the workpiece, and perform flaw detection on the filled cladding area of ​​the workpiece by ultrasonic flaw detection + magnetic particle flaw detection;

[0076] Among them, the results of ultrasonic flaw detection meet the Level 1 standard in GB / T7233.1-2023;

[0077] The results of magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

[0078] Example 4

[0079] The present invention uses ZG20Mn steel castings to manufacture cable clamps for suspension bridges. There are local repair welding parts on the cable clamp structure. The local repair welding parts need to be repaired by surfacing welding. Specifically, the following welding method is used to perform surfacing welding repair and eliminate residual stress defects in the surfacing welding parts, including the following process steps:

[0080] Step 1. The part to be repaired on the workpiece (i.e. the cable clamp structure, the same below) is machined to form a welding groove to form a relatively spacious and easy-to-operate U-shaped welding groove;

[0081] Use a grinding wheel to grind the welding groove on the workpiece to make it smooth, and use the method of penetration testing + magnetic particle flaw detection to test the welding groove on the workpiece to confirm that there are no defects before welding;

[0082] Step 2. Preheat the welding groove area on the workpiece to 170°C;

[0083] Step 3. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the base weld on the welding groove by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 24 L / min, current 260 A, voltage 30 V, current polarity straight reverse, and welding speed 42 cm / min;

[0084] Step 4. To ensure that the adjacent subsequent welds can form a sufficient and dense thermal impact on the base weld and achieve the tempering effect on the coarse grains, the base weld is manually ground from the top side using an angle grinder to remove about 1 / 2 of the thickness of the base weld by grinding;

[0085] Step 5. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the first layer of filler weld on the ground base weld by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 24 L / min, current 280 A, voltage 34 V, current polarity direct and reverse, and welding speed 47 cm / min;

[0086] According to the process that the adjacent previous weld is used as the grinding basis and the next weld is used to heat treat the previous weld, steps 4 and 5 are repeated, that is, after the first-layer filler weld is ground, the second-layer filler weld is welded on the ground first-layer filler weld; after the second-layer filler weld is ground, the third-layer filler weld is welded on the ground second-layer filler weld, and so on, until the welding groove is filled with surfacing;

[0087] Step 6. Use an angle grinder to manually grind the top layer of the filler weld from the top side to remove about 1 / 2 of the thickness of the top layer of the filler weld by grinding;

[0088] Step 7. Use a welding wire with a diameter of 1.2 mm and a grade of ER50-6 to weld the cap layer weld on the top layer of the ground filler cladding by GMAW gas shielded welding. The specific welding parameters are: shielding gas CO2, shielding gas flow rate 24 L / min, current 280 A, voltage 34 V, current polarity direct and reverse, and welding speed 47 cm / min;

[0089] During the welding process of the cap weld, a clearance of about 2.5 mm is required between the edge of the cap weld and the workpiece base material to avoid the formation of a new heat-affected zone between the cap weld and the workpiece base material to generate residual stress defects, that is, the heat-affected zone of the cap weld is only for the top layer of the filler weld.

[0090] Step 8. Use an angle grinder to grind away the excess cladding structure on the welding groove to form a flat structure in the filled cladding area on the workpiece, and perform flaw detection on the filled cladding area of ​​the workpiece by ultrasonic flaw detection + magnetic particle flaw detection;

[0091] Among them, the results of ultrasonic flaw detection meet the Level 1 standard in GB / T7233.1-2023;

[0092] The results of magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

[0093] Based on the welding method of the above-mentioned embodiment 1, a fracture toughness test was carried out, that is, multi-layer tempering welds were welded on the test plate according to the welding method of embodiment 1, and the fracture toughness test was carried out on the test plate, and the CTOD values ​​of the heat affected zone and weld of the welded joint were obtained as shown in Table 1 (note that different sample numbers under the same test item in the table refer to the sampling numbers at different positions along the length direction of the weld at the same surface depth, and the sampling depth and length position under each test item are the same, the same below).

[0094] Table 1 CTOD values ​​of heat affected zone and weld of multi-layer tempered welds of test plate

[0095]

[0096] As a comparison, the fracture toughness test was carried out with the conventional surfacing welding process, and the fracture toughness test was carried out with the conventional surfacing welding process post-weld heat treatment (the post-weld heat treatment process is post-weld heat preservation at 540℃±10℃ for 4 hours). Among them, the test plate obtained by the conventional surfacing welding process is numbered T1, and the test plate obtained by the conventional surfacing welding process post-weld heat treatment is numbered T2. By carrying out fracture toughness tests on the T1 test plate and the T2 test plate, the CTOD values ​​of the heat affected zone and weld of the weld joint as shown in Table 2 were obtained.

[0097] Table 2 CTOD values ​​of heat affected zone and weld of welded joints of T1 test plate and T2 test plate

[0098]

[0099]

[0100] By comparing Table 1 with Table 2, it can be found that the CTOD values ​​of the heat affected zone and weld of the multi-layer tempered weld test plate are not as good as the CTOD values ​​of the heat affected zone and weld of the weld of the conventional surfacing welding process test plate T2 after heat treatment, but are much better than the CTOD values ​​of the heat affected zone and weld of the weld of the conventional surfacing welding process test plate T1 without heat treatment after welding. It can be seen that the multi-layer tempered weld welding method of the present invention can effectively eliminate the residual stress defects of the surfacing layer of the cast steel part, thereby effectively meeting the technical requirements of easy, economical, efficient and high-quality molding of large cast steel structural parts for suspension bridges, and further effectively solving the technical problem of large residual stress of large cast steel structural parts after welding due to lack of suitable stress relief equipment, and the finished product quality is high.

[0101] The above embodiments are only used to illustrate the present invention, but not to limit it.

[0102] Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the above embodiments or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not deviate the essence of the corresponding technical solutions from the spirit and scope of the present invention.

Claims

1. A welding method for eliminating residual stress defects in the cladding layer of a steel casting, characterized in that: The welding method comprises the following process steps: Step 1. Pre-treat the welding groove on the workpiece; Step 2. Preheat the welding groove area to 150-200°C; Step 3. Weld the base weld on the welding groove by gas shielded welding; Step 4. Grind away 1 / 3 to 2 / 3 of the thickness of the base weld from the top side; Step 5. Use gas shielded welding to weld the first filler weld on the ground base weld. The process of using the adjacent previous weld bead as the grinding basis and the subsequent weld bead heat treating the previous weld bead is repeated in steps 4 and 5 until the welding groove is filled with surfacing; Step 6. Grind away 1 / 3 to 2 / 3 of the thickness of the top layer of the filler cladding from the top side; Step 7. Performing a cap layer weld at the topmost layer of the filler cladding in step 6 by means of gas shielded welding, and forming a gap fit between the edge of the cap layer weld and the base material of the workpiece; Step 8. Remove the excess weld structure on the weld groove and perform flaw detection.

2. The welding method for eliminating residual stress defects in the weld overlay of a steel casting according to claim 1, characterized in that: The workpiece base material is ZG20Mn steel casting, and the welding wire used is ER50-6 welding wire with a diameter of 1.2 mm; In step 3, the welding parameters of the base weld are: shielding gas CO2, shielding gas flow rate 20-25 L / min, current 240-300 A, voltage 26-32 V, current polarity direct and reverse, welding speed 35-45 cm / min; In step 5, the welding parameters of the filling layer weld are: shielding gas CO2, shielding gas flow rate 20-25L / min, current 260-320A, voltage 28-36V, current polarity direct and reverse, welding speed 40-50cm / min; In step 7, the welding parameters of the cover layer weld are: shielding gas CO2, shielding gas flow rate 20-25L / min, current 260-320A, voltage 28-36V, current polarity direct and reverse, and welding speed 40-50cm / min.

3. The welding method for eliminating residual stress defects in the weld overlay of a steel casting according to claim 1 or 2, characterized in that: The workpiece is a cable clamp, a cable saddle or a loose cable sleeve for a suspension bridge.

4. The welding method for eliminating residual stress defects in the cladding layer of a steel casting according to claim 1, characterized in that: In step 1, the pretreatment is to grind the welding groove on the workpiece to be smooth and detect to confirm that there are no defects before welding.

5. The welding method for eliminating residual stress defects in the cladding layer of a steel casting according to claim 4, characterized in that: The detection method confirmed by the test is penetration testing + magnetic particle testing.

6. The welding method for eliminating residual stress defects in the weld overlay of a steel casting according to claim 1 or 4, characterized in that: The welding groove on the workpiece is a U-shaped groove.

7. The welding method for eliminating residual stress defects in the cladding layer of a steel casting according to claim 1, characterized in that: The grinding is performed manually using an angle grinder.

8. The welding method for eliminating residual stress defects in the cladding layer of a steel casting according to claim 1, characterized in that: In step 7, the fitting clearance between the edge of the cover layer weld and the workpiece base material is 2 to 3 mm.

9. The welding method for eliminating residual stress defects in the cladding layer of a steel casting according to claim 1, characterized in that: In step 8, the flaw detection method is ultrasonic flaw detection + magnetic particle flaw detection; The ultrasonic flaw detection result meets the Level 1 standard in GB / T7233.1-2023; The results of the magnetic particle inspection meet the Level 1 standard in GB / T 9444-2019.

Citation Information

Cited By

  • Heat-treatment-free repair method for steel casting

    CN120023585A

  • Surfacing process and device for charging bell

    CN120772628A