Firework and cracker mould pressing lump material and preparation method thereof
By using a combination of anhydrous gypsum, tapioca flour, wood fiber and stearic acid to replace traditional stone powder, fireworks and firecracker molded lump materials, the high cost and environmental protection problems of stone powder are solved, and cost reduction, performance improvement and environmental benefits are achieved. win-win.
Patent Information
- Application Number
- CN202411022879.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The high amount of stone powder in existing fireworks and firecracker molded lump materials leads to high production costs and insufficient market competitiveness. Moreover, stone powder mining has an impact on the environment. It is necessary to find alternatives to stone powder to deal with environmental protection issues.
Using anhydrous gypsum, cassava flour, wood fiber, stearic acid and water, the fireworks and firecracker molding material is prepared through heating molding process, reducing the amount of wood fiber and water, and using type II anhydrous gypsum powder to replace stone powder. Optimize molding density and strength.
It reduces production costs, reduces the use of wood fibers and water, improves the strength and lightweight performance of the product. At the same time, the weathering and decomposition of anhydrous gypsum is faster, and the phosphorus-containing element is conducive to plant growth and does not have the risk of combustion. The economic, social and ecological benefits have been improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application belongs to the field of building materials, and in particular relates to a fireworks and firecracker molded lump material and a preparation method thereof. Background Art
[0002] At present, the main raw materials used for molded fireworks and firecrackers are stone powder and cassava flour, and the auxiliary materials are admixtures such as stearic acid and wood fiber. The production process is to mix the raw materials evenly, add hot water (90-100℃) and stir, put them into the mold for extrusion molding, heat and dry, pack and stack, and leave the factory after passing the inspection. The amount of stone powder used is more than 60%, resulting in high production costs and insufficient market competitiveness; in addition, the stone powder used needs to be mined from the mountains, and new substitutes need to be found.
[0003] Therefore, it is urgent to develop a fireworks and firecracker molded lump material that does not require the use of stone powder and has better performance to adapt to the current overall environment where environmental protection issues are increasingly valued. Summary of the invention
[0004] In order to solve the above technical problems existing in the prior art, the present application provides a fireworks and firecrackers molded lump material and a preparation method thereof, which is specifically achieved through the following technical scheme:
[0005] A fireworks and firecrackers molded lump material is composed of the following raw materials: anhydrous gypsum, cassava flour, wood fiber, stearic acid and water.
[0006] Further, the weight proportions of the raw materials are as follows: 800-900 parts of anhydrous gypsum, 100-150 parts of cassava flour, 25-50 parts of wood fiber, 4-7 parts of stearic acid, and 6000-7000 parts of water. Preferably, 795 parts of anhydrous gypsum, 150 parts of cassava flour, 50 parts of wood fiber, 5 parts of stearic acid, and 6500 parts of water.
[0007] Furthermore, the anhydrous gypsum is type II anhydrous gypsum powder.
[0008] The method for preparing the fireworks and firecrackers molded lump material comprises the following steps:
[0009] (1) Material preparation: weigh anhydrous gypsum, tapioca flour, wood fiber, stearic acid, and water according to a weight ratio;
[0010] (2) Mixing: Heat water to 90-100°C, mix other raw materials evenly, add hot water and stir evenly, then add it to the combined mold cavity with a mold temperature of 170-190°C, then close the mold and continue heating to make the temperature inside the mold 190-210°C, so that it is formed and solidified until there is no water vapor coming out of the mold, open the mold and exit the molded lump product.
[0011] Compared with the prior art, the technical effects created by this application are embodied in:
[0012] 1. It can reduce the amount of additives such as wood fiber. Under the same conditions, the anhydrous gypsum molded lump needs about 40-50% less wood fiber than the stone powder molded lump. From this point of view, the cost can be saved by about 50 yuan. (The specific gravity of anhydrous gypsum is lighter than that of stone powder; the bulk density of anhydrous gypsum (750-850㎏ / L 3 ), stone powder bulk density (1400-1500㎏ / L 3 ), and the main purpose of using wood fiber is to reduce weight. When the overall weight is reduced, the amount of wood fiber is also greatly reduced. According to the situation of this application, the amount of wood fiber can be reduced by about 50%. One ton of wood fiber is about 1,000 yuan, so the cost saving is about 50 yuan).
[0013] 2. The water consumption of the new type II anhydrous gypsum powder used in this application is higher than that of stone powder. After heating and molding to evaporate the water, the bulk density of the product is lighter than that of stone powder. The bulk density of anhydrous gypsum (750-850㎏ / L 3 ), stone powder bulk density (1400-1500㎏ / L 3 ), that is, with the same raw materials, anhydrous gypsum and stone powder, the same volume of anhydrous gypsum molded balls are about 5% lighter than the molded balls produced by stone powder.
[0014] 3. Under the same conditions, the new type II anhydrous gypsum powder used in this application is used to replace stone powder, and the strength of the molded product is better than that of the product with stone powder.
[0015] 4. The product of the present application weathers and decomposes quickly. It only takes about 90 days for the molded lumps made of anhydrous gypsum to completely weather and decompose, while the molded lumps made of stone powder cannot be completely decomposed after about 150 days of weathering and decomposition. In addition, the anhydrous gypsum molded lumps in the present application contain weak phosphorus-containing compounds. The phosphorus element in it is beneficial to plant growth after weathering and decomposition, and there is no risk of combustion.
[0016] 5. With the production process unchanged, the key performance indicators of the products produced by the patented formula are improved while the cost is reduced. The raw material of the new type II anhydrous gypsum powder used in this application is industrial solid waste phosphogypsum, which can also dispose of solid waste. The implementation of this patent can achieve significant economic, social and ecological benefits at the same time. DETAILED DESCRIPTION
[0017] The technical solution of the present application is further limited below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0018] Example 1
[0019] A fireworks and firecrackers molded lump material, composed of the following raw materials:
[0020] 81.2kg anhydrous gypsum, 15kg cassava flour, 3kg wood fiber, 0.8kg stearic acid, 60kg water.
[0021] The anhydrous gypsum is type II anhydrous gypsum powder, specifically, anhydrous gypsum obtained by calcining phosphogypsum at 600-800° C. and then grinding and modifying the anhydrous gypsum to obtain a powder material.
[0022] Before use, mix the weighed materials, add 90-100℃ hot water and stir evenly, then add them into the combined mold cavity with a mold temperature of about 180℃, then close the mold and continue heating to make the temperature inside the mold about 200℃, so that it can be formed and solidified until there is no water vapor coming out of the mold, and then open the mold to exit the molded lump product.
[0023] Example 2
[0024] A fireworks and firecrackers molded lump material, composed of the following raw materials:
[0025] 81.8kg anhydrous gypsum, 13kg cassava flour, 4kg wood fiber, 1.2kg stearic acid, 65kg water.
[0026] The anhydrous gypsum is type II anhydrous gypsum powder, specifically, anhydrous gypsum obtained by calcining phosphogypsum at 600-800° C. and then grinding and modifying the anhydrous gypsum to obtain a powder material.
[0027] Before use, mix the weighed materials, add 90-100℃ hot water and stir evenly, then add them into the combined mold cavity with a mold temperature of about 180℃, then close the mold and continue heating to make the temperature inside the mold about 200℃, so that it can be formed and solidified until there is no water vapor coming out of the mold, and then open the mold to exit the molded lump product.
[0028] Example 3
[0029] A fireworks and firecrackers molded lump material, composed of the following raw materials:
[0030] 83kg anhydrous gypsum, 13kg cassava flour, 3kg wood fiber, 1kg stearic acid, 62kg water.
[0031] The anhydrous gypsum is type II anhydrous gypsum powder, specifically, anhydrous gypsum obtained by calcining phosphogypsum at 600-800° C. and then grinding and modifying the anhydrous gypsum to obtain a powder material.
[0032] Before use, mix the weighed materials, add 90-100℃ hot water and stir evenly, then add them into the combined mold cavity with a mold temperature of about 180℃, then close the mold and continue heating to make the temperature inside the mold about 200℃, so that it can be formed and solidified until there is no water vapor coming out of the mold, and then open the mold to exit the molded lump product.
[0033] The performance test results of each embodiment are as follows:
[0034]
[0035]
[0036] Finally, it should be pointed out that the above embodiments are only representative examples of the present application. Obviously, the technical solution of the present application is not limited to the above embodiments, and there may be many variations. All variations that can be directly derived or associated with the contents disclosed in the present application by a person of ordinary skill in the art should be considered as the protection scope of the present application.
Claims
1. A fireworks and firecrackers molded lump material, characterized in that: It is composed of the following raw materials: anhydrous gypsum, cassava flour, wood fiber, stearic acid and water.
2. The fireworks and firecrackers molded lump material according to claim 1, characterized in that: The weight proportions of the raw materials are as follows: 800-900 parts of anhydrous gypsum, 100-150 parts of cassava flour, 25-50 parts of wood fiber, 4-7 parts of stearic acid, and 6000-7000 parts of water.
3. The fireworks and firecrackers molded lump material according to claim 1, characterized in that: The weight proportions of the raw materials are as follows: 795 parts of anhydrous gypsum, 150 parts of cassava flour, 50 parts of wood fiber, 5 parts of stearic acid, and 6500 parts of water.
4. The fireworks and firecrackers molded lump material according to claim 1, characterized in that: The anhydrous gypsum is type II anhydrous gypsum powder.
5. The method for preparing the fireworks and firecracker molded lump material according to claim 1, characterized in that: The steps include: (1) Material preparation: weigh anhydrous gypsum, tapioca flour, wood fiber, stearic acid, and water according to a weight ratio; (2) Mixing: Heat water to 90-100°C, mix other raw materials evenly, add hot water and stir evenly, then add it to the combined mold cavity with a mold temperature of 170-190°C, then close the mold and continue heating to make the temperature inside the mold 190-210°C, so that it is formed and solidified until there is no water vapor coming out of the mold, and then open the mold to withdraw the molded lump product.
Citation Information
Cited By
High-strength firework molded lump body based on in-situ whisker toughening and staged curing and preparation method of high-strength firework molded lump body
CN122281677A