Preparation method of 107 glue and 107 glue
107 glues were prepared by dimethyldichlorosilane hydrolysate and silane small molecules. The polymerization and degradation treatment combined with neutralization treatment, which solved the problems of complex process and high cost in the prior art, and achieved high stability and high yield Preparation of low viscosity 107 glue.
Patent Information
- Application Number
- CN202411323228.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing 107 rubber preparation methods have complex processes, high cost and low product stability, making it difficult to meet the viscosity requirements of high-precision silicone rubber products.
The viscosity is obtained by using dimethyldichlorosilane hydrolysate and silane small molecules as raw materials. The viscosity is reached by polymerization treatment, and then degradation treatment is performed to 2000 ± 200 mPa·s. Combined with neutralization treatment and delow treatment, the viscosity is obtained. 107 glue with 2000±200mPa·s and volatile content is not higher than 0.8%.
The preparation of low viscosity 107 glue is achieved, with high product stability, high yield, short production cycle, low equipment and production costs, and no distillation treatment is required.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical synthesis, and particularly relates to a preparation method of 107 glue and the 107 glue. Background Art
[0002] 107 glue is one of the raw materials for many silicone rubber products, and its application range is very wide. The specifications of 107 glue products are different. The common specifications of 107 glue on the market are 20,000 viscosity, 50,000 viscosity, 80,000 viscosity, etc. The production methods of common viscosities mostly use dimethyl carbonate or dimethyldichlorosilane hydrolyzate as production raw materials, assisted by KOH, tetramethylammonium hydroxide alkaline glue, etc. as catalysts. With the continuous progress of society, most silicone rubber products tend to be high-end, and there are further requirements for the product viscosity of 107 glue, tending to have too high or too low viscosity specifications. At present, the industry mainly produces 107 glue with a viscosity of 1000 to 2000 by distilling the raw materials, but the distillation process greatly prolongs the preparation time of the product and increases the operation and equipment costs.
[0003] Therefore, it is necessary to continue to study the preparation method of 107 glue, so as to obtain 107 glue with low viscosity, high product stability and yield, and reduce production costs. Summary of the invention
[0004] The invention provides a method for preparing 107 glue, which is used to solve the problems of complex process, high cost and low product stability in the prior art when preparing low-viscosity 107 glue.
[0005] The invention provides a 107 glue which is prepared by the method and has lower viscosity and higher product stability and yield.
[0006] In one aspect, the present invention provides a method for preparing 107 glue, comprising the following steps: (1) Mixing a raw material system including dimethyldichlorosilane hydrolyzate and silane small molecules uniformly, and performing a dehydration treatment to obtain a mixture having a water content of no more than 2 ppm; wherein the viscosity of the silane small molecules is 1-2 mm 2 / s; (2) adding a catalyst to the mixture for polymerization to obtain a first polymer having a viscosity of 5000±500 mPa·s; (3) adding water to the first polymer for degradation treatment to obtain a second polymer having a viscosity not higher than 2000±200 mPa·s; (4) neutralizing the second polymer to a pH value of 6.5-7, and then performing a desulfurization treatment to obtain the 107 glue having a viscosity of 2000±200 mPa·s and a volatile matter of not more than 0.8%; wherein the temperature of the desulfurization treatment is not less than 210°C.
[0007] Furthermore, in step (1), the mass ratio of the dimethyldichlorosilane hydrolyzate to the silane small molecule is (4-6):1.
[0008] Furthermore, in step (4), the temperature of the degassing treatment is 210-220°C, the vacuum degree is not higher than 5KPa, and the time is 4-5h.
[0009] Furthermore, in step (1), the temperature of the dehydration treatment is 70-90° C.; and / or, In step (2), the polymerization treatment temperature is 140-160°C and the pressure is -0.07-0 MPa; and / or, In step (3), the temperature of the degradation treatment is 140-160°C.
[0010] Furthermore, in step (3), the amount of water added is 5000-10000 ppm based on the mass of the first polymer.
[0011] Furthermore, in step (2), the catalyst comprises an aqueous solution of potassium hydroxide; and / or, In step (4), phosphoric acid is used as a neutralizing agent to participate in the neutralization treatment.
[0012] Furthermore, the mass fraction of the potassium hydroxide aqueous solution is 40-60%, and the added amount of the potassium hydroxide aqueous solution accounts for 140-160 ppm of the mass of the mixture.
[0013] Furthermore, the phosphoric acid is analytically pure, and the amount of the phosphoric acid added accounts for 224-320 ppm of the mass of the second polymer.
[0014] Furthermore, before step (1), the method further comprises: filtering the dimethyldichlorosilane hydrolyzate.
[0015] On the other hand, the present invention provides a 107 glue, which is prepared by the above-mentioned preparation method to obtain the 107 glue with a viscosity of 2000±200 mPa·s and a volatile matter not higher than 0.8%.
[0016] The invention provides a preparation method of 107 glue. The method comprises the following steps: using dimethyldichlorosilane hydrolyzate and silane small molecules as raw materials, firstly subjecting the raw material system to a polymerization treatment so that the viscosity reaches 5000±500 mPa·s, and then subjecting the raw material system to a degradation treatment so that the viscosity is reduced to a target viscosity, and combining the neutralization treatment and the deoxidation treatment, so as to obtain 107 glue with a viscosity of 2000±200 mPa·s and a volatile matter of not more than 0.8%. The product has stable quality, a mature preparation method, a high yield, no need for distillation treatment of the raw material system, a short production cycle, and low equipment and production costs. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] In one aspect, the present invention provides a method for preparing 107 glue, comprising the following steps: (1) Mixing a raw material system including dimethyldichlorosilane hydrolyzate and silane small molecules uniformly, and performing a dehydration treatment to obtain a mixture having a water content of no more than 2 ppm; wherein the viscosity of the silane small molecules is 1-2 mm 2 / s; (2) adding a catalyst to the mixture for polymerization to obtain a first polymer having a viscosity of 5000±500 mPa·s; (3) adding water to the first polymer for degradation treatment to obtain a second polymer with a viscosity of 2000±200 mPa·s; (4) The second polymer is neutralized to a pH value of 6.5-7, and then depolymerized to obtain a 107 glue having a viscosity of 2000±200 mPa·s and a volatile matter of not more than 0.8%; wherein the depolymerization temperature is not less than 210°C.
[0019] Among them, 107 glue refers to polyvinyl formal adhesive, which is an adhesive formed by a solution or emulsion with water as the medium.
[0020] In step (1), by using dimethyldichlorosilane hydrolyzate and silane small molecules as a raw material system, it is beneficial to prepare a 107 glue product with lower viscosity and reduce the cost of raw materials; wherein the viscosity of dimethyldichlorosilane hydrolyzate is ≤70.00mm 2 / s, its main components include dimethylsiloxane ring and hydroxyl-terminated dimethylsiloxane line; the viscosity of silane small molecules is 1-2mm2 / s, its main components include D4 (octamethylcyclotetrasiloxane), D3 (hexamethylcyclotrisiloxane), D5 (decamethylcyclopentasiloxane), short-chain dimethylsiloxane linear body, etc.
[0021] In step (2), a catalyst is added to cause the raw material system to undergo a polymerization reaction. When the viscosity of the polymer system is 5000±500 mPa·s, the polymerization reaction is stopped to obtain a first polymer. The viscosity is measured in real time by an online viscometer.
[0022] In step (3), water is added to the first polymer having a viscosity of 5000±500 mPa·s to perform a degradation treatment so as to reduce the viscosity of the polymer. The viscosity change is observed by an online viscometer. When the viscosity of the polymer is 2000±200 mPa·s, the degradation treatment is stopped to obtain a second polymer.
[0023] In step (4), the second polymer that has reached the target viscosity is neutralized until the pH value of the second polymer is 6.5-7, thereby neutralizing the catalyst added in step (2). At this time, the system cannot continue to undergo polymerization reaction, and then a desulfurization treatment is performed at a temperature not lower than 210° C. to further remove small molecular substances in the system, thereby obtaining 107 glue with a viscosity not higher than 2200 mPa·s and a volatile matter not higher than 0.8%.
[0024] The invention provides a preparation method of 107 glue. The method comprises the following steps: using dimethyldichlorosilane hydrolyzate and silane small molecules as raw materials, firstly subjecting the raw material system to a polymerization treatment so that the viscosity reaches 5000±500 mPa·s, and then subjecting the raw material system to a degradation treatment so that the viscosity is reduced to a target viscosity, and combining the neutralization treatment and the deoxidation treatment, so as to obtain 107 glue with a viscosity of 2000±200 mPa·s and a volatile matter of not more than 0.8%. The product has stable quality, a mature preparation method, a high yield, no need for distillation treatment of the raw material system, a short production cycle, and low equipment and production costs.
[0025] The present invention does not limit the equipment used in the preparation method, and any equipment that can provide the temperature and pressure required by the method can be used; in a specific embodiment, the above preparation method is carried out using a polymerization kettle.
[0026] In a specific embodiment, the small molecule substances obtained by dehydration treatment are used as silane small molecules in the raw material system to participate in dehydration treatment, which can further recover the raw materials and reduce costs.
[0027] Furthermore, in step (1), the mass ratio of dimethyldichlorosilane hydrolyzate to silane small molecules is (4-6):1.
[0028] By controlling the mass ratio of dimethyldichlorosilane hydrolyzate and silane small molecules in the raw material system, the yield of 107 glue can be further improved, the viscosity of the product can be further controlled, and the volatile content can be reduced.
[0029] Furthermore, in step (4), the temperature of the degassing treatment is 210-220°C, the vacuum degree is 3-5 KPa, and the time is 4-5 hours.
[0030] By further limiting the temperature and vacuum degree of the degassing treatment, small molecular substances can be further removed, the yield of 107 glue can be increased, and the volatile content can be reduced.
[0031] In one specific embodiment, in step (1), the temperature of the dehydration treatment is 70-90°C.
[0032] In another specific embodiment, in step (2), the polymerization treatment temperature is 140-160° C. and the pressure is -0.07-0 MPa.
[0033] In another specific embodiment, in step (3), the temperature of the degradation treatment is 140-160° C. and the pressure is normal pressure.
[0034] By limiting the specific execution parameters of each step, the yield of 107 glue can be further improved, the viscosity of the product can be further controlled, and the volatile content can be reduced.
[0035] Specifically, the pressure of the polymerization treatment can be achieved by adjusting the opening of the valve at the steam outlet of the polymerization reactor.
[0036] Optionally, in step (3), the amount of water added is 5000-10000 ppm based on the mass of the first polymer.
[0037] By limiting the amount of water added, the polymer viscosity can be further controlled to reach the target viscosity, the yield of 107 glue can be further improved, the product viscosity can be further controlled, the volatile content can be reduced, and energy consumption can be further saved.
[0038] Optionally, in step (2), the catalyst comprises an aqueous solution of potassium hydroxide.
[0039] The raw material system is polymerized by using potassium hydroxide aqueous solution as a catalyst, so that the preparation method is simpler, the raw materials are easy to obtain, the production cost can be further saved, and the subsequent neutralization treatment is more conducive to achieving better results.
[0040] In step (4), phosphoric acid is used as a neutralizing agent to participate in the neutralization treatment.
[0041] Specifically, the mass fraction of the potassium hydroxide aqueous solution is 40-50%, and the added amount of the potassium hydroxide aqueous solution accounts for 140-160 ppm of the mass of the mixture.
[0042] Phosphoric acid is of analytical grade, and the amount of phosphoric acid added is 224-320 ppm based on the mass of the second polymer.
[0043] By further limiting the mass fraction and addition amount of the reagents, the yield of 107 glue can be further improved, the viscosity of the product can be further controlled, and the volatile content can be reduced.
[0044] Furthermore, before step (1), the method further comprises: filtering the dimethyldichlorosilane hydrolyzate.
[0045] Impurities in the dimethyldichlorosilane hydrolyzate can be removed by filtering, making the raw material purity higher, further improving the yield of 107 glue, further controlling the product viscosity and reducing the volatile content.
[0046] On the other hand, the present invention also provides a 107 glue, which is prepared by the above-mentioned preparation method to obtain a 107 glue with a viscosity of 2000±200mPa·s and a volatile matter of no more than 0.8%.
[0047] The 107 glue provided by the invention has lower viscosity and volatile matter.
[0048] The following is a detailed introduction to the preparation method of 107 glue provided by the present invention through specific examples. Example 1
[0049] The preparation method of 107 glue used in this embodiment includes the following steps: (1) The hydrolyzate of dimethyldichlorosilane (viscosity ≤ 70 mm) with a mass ratio of 4:1 is added. 2 / s) and silane small molecules (viscosity 1-2mm 2 / s) of the raw material system is added into the polymerization kettle and mixed evenly, and dehydrated at 90°C for 60 minutes to obtain a mixture with a water content of no more than 2ppm; (2) adding 140 ppm of a catalyst (a 50% by mass potassium hydroxide aqueous solution) to the mixture, and polymerizing the mixture at 160° C. and −0.05 KPa for 3 h to obtain a first polymer having a viscosity of 5000 mPa·s; (3) adding 5000 ppm of water to the first polymer and performing degradation treatment at 150° C. and normal pressure to obtain a second polymer having a viscosity of 2200 mPa·s; (4) The second polymer was neutralized by adding 224 ppm of a neutralizing agent until the pH value reached 6.5; the second polymer was then degased at 200°C and a vacuum degree of 4 KPa for 4.5 hours to obtain 107 glue. Example 2
[0050] The difference between this embodiment and embodiment 1 is that in step (1), the temperature of the dehydration treatment is 80°C. Example 3
[0051] The difference between this embodiment and embodiment 1 is that in step (1), the temperature of the dehydration treatment is 70°C. Example 4
[0052] The difference between this embodiment and embodiment 1 is that in step (1), the temperature of the dehydration treatment is 65°C. Example 5
[0053] The difference between this embodiment and embodiment 1 is that in step (1), in the raw material system, the mass ratio of dimethyldichlorosilane hydrolyzate to silane small molecules is 7:1. Example 6
[0054] The difference between this embodiment and embodiment 1 is that in step (2), the temperature of the polymerization treatment is 150°C. Example 7
[0055] The difference between this embodiment and embodiment 1 is that in step (2), the temperature of the polymerization treatment is 140°C. Example 8
[0056] The difference between this embodiment and embodiment 1 is that in step (2), the temperature of the polymerization treatment is 135°C. Example 9
[0057] The difference between this embodiment and embodiment 1 is that in step (2), the temperature of the polymerization treatment is 165°C. Example 10
[0058] The difference between this embodiment and embodiment 1 is that in step (2), the amount of catalyst added is 160 ppm. Embodiment 11
[0059] The difference between this embodiment and embodiment 1 is that in step (2), the amount of catalyst added is 135 ppm. Example 12
[0060] The difference between this embodiment and embodiment 1 is that in step (2), the polymerization treatment time is 2 hours, and the first polymer with a viscosity of 4800 mPa·s is obtained. Example 13
[0061] The difference between this embodiment and embodiment 1 is that in step (2), the polymerization treatment time is 4 hours, and the first polymer with a viscosity of 5200 mPa·s is obtained. Embodiment 14
[0062] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 5200 ppm. Embodiment 15
[0063] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 5500 ppm. Example 16
[0064] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 7000 ppm. Embodiment 17
[0065] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 7500 ppm. Embodiment 18
[0066] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 8000 ppm. Embodiment 19
[0067] The difference between this embodiment and embodiment 1 is that in step (3), the amount of water added is 11000 ppm. Embodiment 20
[0068] The difference between this embodiment and embodiment 1 is that in step (4), the amount of the neutralizing agent added is 320 ppm. Embodiment 21
[0069] The difference between this embodiment and embodiment 1 is that in step (4), the amount of the neutralizing agent added is 350 ppm. Embodiment 22
[0070] The difference between this embodiment and embodiment 1 is that in step (4), the temperature of the desulfurization treatment is 200° C. and the vacuum degree is 2 KPa. Embodiment 23
[0071] The difference between this embodiment and embodiment 1 is that in step (4), the time of the desalination treatment is 3.5 hours.
[0072] Comparative Example 1 The difference between this comparative example and Example 1 is that in step (1), no silane small molecule is added.
[0073] Comparative Example 2 The difference between this comparative example and Example 1 is that in step (2), the polymerization treatment obtains a first polymer with a viscosity of 6000 mPa·s.
[0074] Comparative Example 3 The difference between this comparative example and Example 1 is that in step (2), the polymerization treatment is performed to obtain a first polymer with a viscosity of 2000 mPa·s, and step (3) is not performed.
[0075] Comparative Example 4 The difference between this comparative example and Example 1 is that in step (4), the temperature of the desulfurization treatment is 180°C.
[0076] Test Example 1 The 107 glue prepared in the above embodiments and comparative examples was tested, and the results are shown in Table 1.
[0077] Among them, the viscosity is obtained by online viscosity meter testing; The volatile matter is obtained by testing in an electric blast drying oven, and the calculation formula is:
[0078]
[0079] The invention provides a preparation method of 107 glue. The method comprises the following steps: using dimethyldichlorosilane hydrolyzate and silane small molecules as raw materials, firstly subjecting the raw material system to a polymerization treatment so that the viscosity reaches 5000±500 mPa·s, and then subjecting the raw material system to a degradation treatment so that the viscosity is reduced to a target viscosity, and combining the neutralization treatment and the deoxidation treatment, so as to obtain 107 glue with a viscosity of 2000±200 mPa·s and a volatile matter of not more than 1%. The product has stable quality, a mature preparation method, a high yield, no need for distillation treatment of the raw material system, a short production cycle, and low equipment and production costs.
[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein by equivalents. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the protection scope of the present invention.
Claims
1. A method for preparing 107 glue, characterized in that: The following steps are involved: (1) Mixing a raw material system including dimethyldichlorosilane hydrolyzate and silane small molecules uniformly, and performing a dehydration treatment to obtain a mixture having a water content of no more than 2 ppm; wherein the viscosity of the silane small molecules is 1-2 mm 2 / s; (2) adding a catalyst to the mixture for polymerization to obtain a first polymer having a viscosity of 5000±500 mPa·s; (3) adding water to the first polymer for degradation treatment to obtain a second polymer having a viscosity not higher than 2000±200 mPa·s; (4) neutralizing the second polymer to a pH value of 6.5-7, and then performing a desulfurization treatment to obtain the 107 glue having a viscosity of 2000±200 mPa·s and a volatile matter of not more than 0.8%; wherein the temperature of the desulfurization treatment is not less than 210°C.
2. The method for preparing 107 glue according to claim 1, characterized in that: In step (1), the mass ratio of the dimethyldichlorosilane hydrolyzate to the silane small molecule is (4-6):
1.
3. The method for preparing 107 glue according to claim 2, characterized in that: In step (4), the temperature of the degassing treatment is 210-220°C, the vacuum degree is not higher than 5KPa, and the time is 4-5h.
4. The method for preparing 107 glue according to claim 3, characterized in that: In step (1), the temperature of the dehydration treatment is 70-90°C; and / or, In step (2), the polymerization treatment temperature is 140-160°C and the pressure is -0.07-0 MPa; and / or, In step (3), the temperature of the degradation treatment is 140-160°C.
5. The method for preparing 107 glue according to claim 4, characterized in that: In step (3), the amount of water added is 5000-10000 ppm based on the mass of the first polymer.
6. The method for preparing 107 glue according to claim 5, characterized in that: In step (2), the catalyst comprises an aqueous solution of potassium hydroxide; and / or, In step (4), phosphoric acid is used as a neutralizing agent to participate in the neutralization treatment.
7. The method for preparing 107 glue according to claim 6, characterized in that: The mass fraction of the potassium hydroxide aqueous solution is 40-60%, and the added amount of the potassium hydroxide aqueous solution accounts for 140-160 ppm of the mass of the mixture.
8. The method for preparing 107 glue according to claim 7, characterized in that: The phosphoric acid is analytically pure, and the amount of the phosphoric acid added accounts for 224-320 ppm of the mass of the second polymer.
9. The method for preparing 107 glue according to any one of claims 1 to 8, characterized in that: Before step (1), the method further comprises: filtering the dimethyldichlorosilane hydrolyzate.
10. A 107 glue prepared by the preparation method of the 107 glue according to any one of claims 1 to 9, characterized in that: The 107 glue having a viscosity of 2000±200 mPa·s and a volatile matter not higher than 0.8% is obtained.