Metal organic framework material, preparation method and application of metal organic framework material in photodynamic sterilization

The synthesis of scandium metal organic framework materials is assisted by liquid anode glow discharge technology, which solves the problems of cumbersome synthesis steps and poor photostability of photosensitizers in the prior art, and achieves the preparation of metal organic framework materials with high efficiency and low energy consumption and photodynamic sterilization effect. The photocatalytic oxidation capacity and bactericidal rate are significantly improved.

CN118955933AActive Publication Date: 2024-11-15SICHUAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411165855.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The preparation methods of existing metal organic skeleton materials have problems such as cumbersome operation, high energy consumption, long synthesis time and large reagent consumption. In addition, traditional photosensitizers have poor photostability, difficulty in deep tissue treatment, and have normal tissues. Photodamage risk.

Method used

Use liquid anode glow discharge technology to assist in the synthesis of scandium metal organic framework materials, accelerate material formation through microplasma treatment, simplify synthesis steps and improve photocatalytic capacity, combine transition metals in porphyrin rings to enhance photocatalytic efficiency, and in visible light Work within the area to achieve efficient sterilization.

Benefits of technology

It realizes small size, low energy consumption, simple and fast synthesis of metal organic framework materials, significantly improves the photocatalytic oxidation capacity, and can achieve more than 99% pathogenic bacteria at extremely low doses and low radiation, and avoids Complex post-modification process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955933A_ABST
    Figure CN118955933A_ABST
Patent Text Reader

Abstract

The invention discloses a metal organic framework material, a preparation method and application of the metal organic framework material in photodynamic sterilization, and relates to the technical field of biological medicines.The preparation method comprises the steps that meso-tetra (4-carboxyphenyl) porphin is added into N, N-dimethylformamide to be dissolved, and a solution A is obtained; scandium chloride hexahydrate is added into ultrapure water to be dissolved, and a solution B is prepared; mixing the prepared solution A and the prepared solution B, performing ultrasonic treatment, and fully mixing the two solutions to prepare a mixed solution; performing micro-plasma treatment on the mixed solution; and carrying out centrifugal treatment on the mixed solution subjected to the micro-plasma treatment to obtain a metal organic framework solid. According to the invention, a large amount of high-energy electrons are provided in the discharge process by using micro-plasma treatment, rapid deprotonation of the organic linker is promoted, and the method has the advantages of small size, low energy consumption, simplicity, rapidness, green reagent and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedicine technology, and in particular to a metal organic framework material, a preparation method and application thereof in photodynamic sterilization. Background Art

[0002] Pathogenic microorganisms such as bacteria and viruses pose a constant threat to human health. Consuming spoiled food or water contaminated with pathogenic bacteria can cause short-term illnesses (such as diarrhea and headaches), and sometimes even cancer, so it is extremely important to control the growth of these pathogens. Currently, antibiotics are widely used in medicine and animal husbandry. However, excessive use of antibiotics can lead to drug resistance in pathogenic bacteria, which greatly affects sterilization and disease treatment. Therefore, it is very important to develop non-drug-based antimicrobial agents or strategies.

[0003] In recent years, photodynamic therapy (PDT) has attracted much attention in the medical and environmental fields due to its advantages such as high efficiency, broad-spectrum antibacterial and no drug resistance. During the treatment process, photosensitizer (PS) is excited by light to produce reactive oxygen species (ROS) through intersystem crossing (ISC), including singlet oxygen ( 1 O2). However, the existing traditional photosensitizers still have many shortcomings, for example, 1) the structure generally contains conjugated π electron macrocycles, which are very prone to self-aggregation quenching, which leads to poor photostability and seriously affects their photocatalytic ability as photosensitizers, resulting in poor therapeutic effects; 2) some photosensitizers require shorter wavelength light for excitation, and the penetration depth of these short-wavelength light sources is limited, making it inconvenient to treat deep tissue lesions; 3) to solve the difficulty of PS penetrating into the cell membrane, functional groups or cationic groups are introduced into the PS structure, which requires complex synthetic methods and cumbersome operation steps; 4) the production of ROS by traditional photosensitizers depends on the time, intensity and concentration of light source excitation, but high concentration, excessive irradiation time and intensity will inevitably cause a certain degree of photodamage to normal tissues. Therefore, it is urgent to develop a sterilization strategy with simple probe synthesis, working within the phototherapy window (650-800 nm), short irradiation time, low intensity and high efficiency.

[0004] Porphyrin and its derivatives are a class of photosensitive organic molecules with a wide optical absorption range in the visible light region. Adding porphyrin as a structural unit to metal organic frameworks (MOFs) can solve the problem of self-aggregation and maximize its photophysical properties of generating ROS. In addition, the introduction of certain transition metals in the porphyrin ring can also enhance the ISC process and thus improve the photocatalytic ability. However, the existing MOF materials based on porphyrin organic molecules as ligands (such as the PCN series) are prone to rapid electron-hole recombination, which requires combination with other functional materials to form heterostructured photocatalysts to promote the charge transfer of photoelectrons. This requires multi-step synthesis strategies and complex post-modification and / or post-doping methods, which have the disadvantages of cumbersome operation, high energy consumption, long synthesis time, and large reagent consumption. Therefore, it is urgent to develop a method with green reagents, simple and fast synthesis, and low energy consumption for MOF synthesis and efficient sterilization. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for preparing a metal organic framework material, which is used to solve the disadvantages of the multi-step synthesis strategy and complex post-modification and / or post-doping methods in the prior art for preparing metal organic framework materials, such as complicated operation, high energy consumption, long synthesis time and large reagent consumption.

[0006] The present invention is achieved through the following technical scheme. A preparation method of a metal organic framework material comprises: adding meso-tetrakis (4-carboxyphenyl) porphine into N,N-dimethylformamide for dissolution to prepare a solution A; adding scandium chloride hexahydrate into ultrapure water for dissolution to prepare a solution B; the molar ratio of the solution A to the solution B is 1:1, the prepared solution A and the solution B are mixed, and ultrasonic treatment is performed for 2 minutes to fully mix the two solutions to prepare a mixed solution, and the mixed solution is subjected to microplasma treatment for a treatment time of 45 to 60 minutes; the mixed solution after the microplasma treatment is centrifuged to obtain a metal organic framework solid.

[0007] Furthermore, the preparation method may also include washing and precipitating the metal organic framework solid, and freeze-drying the precipitate in a vacuum freeze dryer; and adding ultrapure water to the precipitate obtained after freeze drying to prepare a 0.5 mg / mL solution, and storing it in an environment of 0~4°C.

[0008] Furthermore, washing the precipitate includes washing the precipitate with N,N-dimethylformamide and ethanol three times.

[0009] Furthermore, the freeze-drying time is 12 to 24 h.

[0010] Furthermore, the plasma treatment may include: completely immersing a platinum electrode as an anode in the mixed solution; placing a hollow stainless steel tube 3 to 5 mm above the liquid surface of the mixed solution, and blowing argon gas from the bottom of the hollow stainless steel tube into the liquid surface at a rate of 100 mL / min; using a plasma discharge module, applying a 7V input voltage, so that a micro plasma is formed between the mixed solution and the bottom of the stainless steel tube, and the discharge is continued for 45 to 60 minutes.

[0011] Furthermore, the centrifugation treatment includes a centrifuge speed of 10000-12000 rpm and a centrifugation time of 20-30 min.

[0012] Another aspect of the present invention provides a metal organic framework material. The metal organic framework material is prepared according to the method described above.

[0013] Finally, the present invention provides an application of a metal organic framework material in photodynamic sterilization. The metal organic framework material is prepared by the method described above and used in photodynamic sterilization.

[0014] Furthermore, in photodynamic sterilization, the amount of metal-organic framework material added is 5~20 μg / mL.

[0015] Furthermore, the wavelength of the irradiated light is 420-660 nm, and the irradiation intensity is 12 mW / cm 2 , the irradiation time is 10 min.

[0016] Furthermore, the pathogenic bacteria killed are Escherichia coli and Staphylococcus aureus.

[0017] Furthermore, the killing rate of pathogenic bacteria by photodynamic sterilization is 99~100%.

[0018] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0019] 1. The present invention uses liquid anode glow discharge technology to provide a large number of high-energy electrons during the discharge process, promoting the rapid deprotonation of organic linkers, thereby accelerating the formation of metal organic framework materials (MOF). Compared with traditional metal organic framework material (MOF) synthesis methods such as solvothermal method, microwave-assisted synthesis method, etching method, etc., this technology has the advantages of small size, low energy consumption, simple and fast, and green reagents.

[0020] 2. The present invention also accelerates the process of metal entering the porphyrin ring in liquid anode glow discharge (SAGD), promotes the formation of multi-site metal organic framework materials (MOF), and significantly improves the photocatalytic oxidation ability based on the special properties of scandium (Sc), thereby avoiding complex and tedious post-modification processes. The liquid anode glow discharge (SAGD) microplasma technology is used to assist the synthesis of scandium metal organic frameworks, which has the advantages of simple operation, fast synthesis speed and low energy consumption.

[0021] 3. The present invention uses the synthesized highly porphyrin-metallated Sc-TCPP MOF in photodynamic sterilization, which can achieve photodynamic sterilization at extremely low doses (5-10 μg / mL) and low irradiance (12 mW / cm 2 ) and low illumination time (10 min), and the sterilization rate can reach more than 99%. In addition, due to the wide ultraviolet absorption characteristics of MOF in the visible light region, it can achieve a certain degree of inactivation of bacteria under multiple wavelengths of light. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0023] Figure 1 This is a method flow chart of exemplary embodiment 1 of the present invention.

[0024] Figure 2 Schematic diagram of the synthesis of scandium metal organic framework by microplasma treatment in Example 1 of the present invention.

[0025] Figure 3 This is a scanning electron microscope image of the scandium metal organic framework (Sc-TCPP MOF) in Example 1 of the present invention.

[0026] Figure 4 This is a transmission electron microscope image of the scandium metal organic framework (Sc-TCPP MOF) in Example 1 of the present invention.

[0027] Figure 5 This is an EPR spectrum diagram of singlet oxygen generated by light excitation of the scandium metal organic framework under neutral conditions in Example 2 of the present invention.

[0028] Figure 6 This is a photograph of a Staphylococcus aureus agar plate treated with a scandium metal organic framework solution in Example 2 of the present invention.

[0029] Figure 7 This is the survival rate of Staphylococcus aureus obtained after being treated with the scandium metal organic framework solution in Example 2 of the present invention.

[0030] Figure 8 This is a photo of an Escherichia coli agar plate treated with the scandium metal organic framework solution in Example 2 of the present invention.

[0031] Fig. 9 This is the survival rate of Escherichia coli obtained after being treated with the scandium metal organic framework solution in Example 2 of the present invention.

[0032] Fig.10 These are photos of the Staphylococcus aureus agar plate treated with the scandium metal organic framework solution at different wavelengths in Example 3 of the present invention.

[0033] Fig.11 The survival rate of Staphylococcus aureus treated with the scandium metal organic framework solution at different wavelengths in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0035] Unless otherwise specified, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art in the art to which the present invention relates. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail. Regarding the "comprising", "including", "having", "containing", etc. used herein, they are all open-ended terms, that is, they mean including but not limited to. Unless the context clearly indicates otherwise, the expressions "a" and "one" used herein include plural references. For example, referring to "a cell" includes a plurality of such cells and equivalents known to those skilled in the art, etc. The term "about" used herein means a range of ±20% of the value thereafter. In some embodiments, the term "about" means a range of ±10% of the value thereafter. In some embodiments, the term "about" means a range of ±5% of the value thereafter.

[0036] Example embodiment 1.

[0037] Figure 1 The method flow chart of this exemplary embodiment is shown, and this exemplary embodiment provides a method for preparing a metal organic framework material. Specifically, it includes the following steps:

[0038] Step 1: Add meso-tetrakis(4-carboxyphenyl)porphine into N,N-dimethylformamide for dissolution to prepare solution A.

[0039] Specifically, 87.5 mg of TCPP was dissolved in 17 mL of DMF.

[0040] Step 2: Add scandium chloride hexahydrate into ultrapure water and dissolve it to prepare solution B.

[0041] Specifically, 28.7 mg of scandium chloride hexahydrate was dissolved in 3 mL of ultrapure water.

[0042] Step 3: Mix the prepared solution A and solution B, and use ultrasonic treatment to fully mix the two solutions to prepare a mixed solution. The molar ratio of the two solutions after being fully mixed is 1:1.

[0043] Specifically, the ultrasonic treatment time was 2 min and the ultrasonic frequency was 40 Hz.

[0044] Step 4: The mixed solution is subjected to microplasma treatment for 45 to 60 minutes.

[0045] Specifically, microplasma treatments can include:

[0046] A platinum electrode as an anode was completely immersed in the mixed solution.

[0047] A hollow stainless steel tube was placed 3-5 mm above the liquid surface of the mixed solution, and argon gas was blown into the liquid surface from the bottom of the hollow stainless steel tube at a rate of 100 mL / min.

[0048] Using a plasma discharge module, an input voltage of 7 V was applied to form a micro plasma between the mixed solution and the bottom of the stainless steel tube, and the discharge lasted for 45 to 60 minutes.

[0049] Step 5: Centrifuge the mixed solution after microplasma treatment to obtain a metal organic framework solid.

[0050] Specifically, during the centrifugation process, the centrifuge speed is 10000~12000 rpm, and the centrifugation time is 20~30 min.

[0051] Step 6: Wash and precipitate the metal organic framework solid, freeze-dry the precipitate in a vacuum freeze dryer, and add ultrapure water to the precipitate obtained after freeze drying to prepare a 0.5 mg / mL solution, and store it in an environment of 0~4 ℃.

[0052] Specifically, the MOF solid was washed with dimethylformamide and ethanol three times before precipitation, and the freeze-drying time was 12 to 24 h.

[0053] Example 2:

[0054] In this embodiment, a metal organic framework material is used in photodynamic sterilization. The metal organic framework solution prepared according to the steps in exemplary embodiment 1 is added to the diluted bacterial suspension in an amount of 5-20 μg / mL.

[0055] Then the wavelength was 420~660 nm and the irradiation intensity was 12 mW / cm2 for 10 min.

[0056] Specifically, the bacterial suspension was prepared by placing Escherichia coli and Staphylococcus aureus in 2.5% LB liquid medium, respectively, and incubating them on a shaking shaker at 37°C for 12 h.

[0057] In order to better understand a metal organic framework material, a preparation method and its application in photodynamic sterilization provided in this exemplary embodiment, the content of this method is further explained below in conjunction with the accompanying drawings and examples.

[0058] Embodiment 1,

[0059] In this example, 2,6,6-tetramethylpiperidine (TEMP) and scandium chloride hexahydrate were purchased from Aladdin Biochemical Technology Co., Ltd. (Shanghai, China); N,N-dimethylformamide (DMF), ethanol, hydrochloric acid and tris(hydroxymethyl)aminomethane (Tris) were purchased from Chengdu Cologne Chemical Co., Ltd. (Chengdu, China); tetrakis(4-carboxyphenyl)porphine (TCPP) was purchased from MacLean Biochemical Technology Co., Ltd. (Shanghai, China).

[0060] The steps of synthesizing the metal organic framework solution include:

[0061] Weigh 87.5 mg of TCPP and completely dissolve it in 17 mL of DMF solution to obtain solution A.

[0062] Weigh 28.7 mg of scandium chloride hexahydrate and completely dissolve it in 3 mL of ultrapure water to obtain solution B.

[0063] Solution A and solution B were mixed in a 50 mL glass reactor for micro plasma treatment.

[0064] Specifically, the microplasma treatment includes placing a hollow stainless steel tube about 3 mm above the surface of the mixed solution, blowing argon gas into the liquid surface from the bottom of the stainless steel tube at a rate of 100 mL / min, and a platinum electrode as an anode fully immersed in the solution.

[0065] A DP-GB 15 kV-ignition type (Guangao Electronics, China) was used as the plasma discharge module. After applying an input voltage of 7 V, micro plasma was formed between the solution and the bottom of the stainless steel tube.

[0066] After continuous discharge for 45 min, the mixture was centrifuged at 10,000 rpm for 20 min to obtain a precipitate, which is the metal organic framework.

[0067] The precipitate was washed three times with N,N-dimethylformamide (DMF) and ethanol to remove residual TCPP and scandium ions (Sc 3+ ).

[0068] Finally, the washed precipitate was dried in a vacuum freeze dryer for 12 h, and the freeze-dried precipitate was added to ultrapure water to prepare a 0.5 mg / mL metal organic framework solution, and the solution was stored in a 0-4 °C refrigerator for later use.

[0069] Figure 2 The schematic diagram of the synthesis of scandium metal organic framework by micro plasma treatment in this embodiment is shown. It can be seen from the figure that

[0070] Schematic diagram of the synthesis of scandium (Sc) metal organic framework (Sc-TCPP MOF) by microplasma treatment. The continuous introduction of argon in the system not only provides sufficient non-oxidizing gas atmosphere, but also blows a large amount of active substances generated by microplasma at the gas-liquid interface into the liquid surface. The large amount of high-energy electrons generated in the solution will deprotonate the organic linker (TCPP), promote the combination of Sc and TCPP, and accelerate the formation of MOF. At the same time, microplasma treatment not only promotes the growth and formation of MOF crystal structure, but also accelerates the entry of Sc into the porphyrin ring of TCPP, and finally realizes the preparation of multi-site, porphyrin metallized scandium metal organic framework (Sc-TCPP MOF).

[0071] Figure 3 A scanning electron microscope image of a scandium metal organic framework (Sc-TCPP MOF) produced by the steps in this example is shown. Figure 4 The transmission electron microscope image of the scandium metal organic framework (Sc-TCPP MOF) prepared by the steps in this embodiment is shown. It can be seen from the image that the scandium metal organic framework synthesized by microplasma treatment presents a cubic configuration.

[0072] As can be seen from this embodiment, with the development of microplasma technology, it has made rapid progress in assisting the synthesis of functional nanomaterials. Among them, liquid anode glow discharge (SAGD) technology provides a large number of high-energy electrons during the discharge process, promoting the rapid deprotonation of organic linkers, thereby accelerating the formation of MOF. Compared with traditional MOF synthesis methods such as solvothermal method, microwave-assisted synthesis method, and etching method, this technology has the advantages of small size, low energy consumption, simple and fast, and green reagents. In addition, this method can accelerate the process of metal entering the porphyrin ring, promote the formation of multi-site MOF, and significantly improve the photocatalytic oxidation ability based on the special properties of Sc, which greatly avoids the complex and cumbersome post-modification process, and Sc has two chemical forms in MOF, both as a metal node of the skeleton structure and coordinated with N atoms in the porphyrin ring. The multi-metal site significantly improves the photosensitivity of MOF, which shows that it has a good effect in photodynamic sterilization.

[0073] Embodiment 2,

[0074] The metal organic framework solution used in this example was prepared according to the method described in Example 1.

[0075] In this example, experiments were conducted on Escherichia coli and Staphylococcus aureus to verify the use of metal organic frameworks in photodynamic sterilization.

[0076] First, the prepared scandium metal organic framework is tested for the generation of singlet oxygen under light excitation under neutral conditions. The following steps are performed to obtain:

[0077] First, prepare the buffer solution. Weigh 0.4846 g Tris solid into 50 mL ultrapure water, gradually add 50-fold hydrochloric acid dilution, stir evenly, read the pH value of the solution with a pH meter, and repeat the operation until the pH of the solution stabilizes at 7.0. Prepare 100 mmol / L Tris-HCl buffer solution with pH = 7 and collect it for later use.

[0078] Using TEMP in aqueous solution as 1 As an O2 capture agent, 10 μL of TEMP was added to 200 μL of a mixture of MOF (10 μg / mL) and buffer (Tris-HCl, pH=7).

[0079] Then, the samples were irradiated with a 420 nm LED lamp (3 V, 3 W) for 15 s, 60 s, 120 s, and 180 s, respectively. After the illumination, the samples were immediately placed in an EPR spectrometer to detect the reactive oxygen species and their production. Figure 5 As shown, Figure 5The EPR spectrum of singlet oxygen produced by the scandium metal organic framework under neutral conditions is shown. As can be seen from the figure, as the illumination time increases, the production of singlet oxygen also increases. Singlet oxygen ( 1 O2) has strong oxidizing properties and can be used for sterilization. As a highly reactive reactive oxygen species (ROS), it can react with unsaturated fatty acids in the cell membrane, causing lipid peroxidation, thereby destroying the integrity and function of the cell membrane, and can oxidize amino acid residues in proteins, especially sulfur-containing amino acids, leading to protein denaturation and enzyme inactivation. The singlet oxygen generated by the photodynamic process can effectively kill pathogenic bacteria.

[0080] In summary, the scandium metal organic framework prepared in the present invention has a bactericidal effect. The following will further illustrate the killing effect of the scandium metal organic framework on common Escherichia coli and Staphylococcus aureus through experiments.

[0081] First, prepare the culture medium for culturing Escherichia coli and Staphylococcus aureus:

[0082] Weigh 5 g of LB broth into 200 mL of ultrapure water and stir to dissolve evenly to obtain liquid culture medium.

[0083] Weigh 25 g of LB broth into 1000 mL of ultrapure water, add 15 g of agar powder, and stir in a 60°C water bath to dissolve evenly to obtain a solid culture solution.

[0084] The culture medium was then sterilized in an autoclave at 121°C for 20 min.

[0085] After the culture medium was prepared, Escherichia coli and Staphylococcus aureus were placed in 2.5% LB liquid culture medium respectively and incubated on a shaking shaker at 37°C for 12 h.

[0086] Afterwards, the bacterial suspension was diluted to 10 6 times, and mixed with different volumes of ScMOF solution. Specifically, the final concentrations of ScMOF solution for treating Staphylococcus aureus were 5, 10, and 20 μg / mL; the final concentrations of ScMOF solution for treating Escherichia coli were 1, 5, and 10 μg / mL.

[0087] Then, a 420 nm LED light (12 mW / cm 2 ) for 10 minutes.

[0088] Next, 60 μL of the treated bacterial solution was spread on a plate containing 1.5% agar and 2.5% LB broth, and the plate was evenly spread using a glass spreading rod sterilized with an alcohol lamp.

[0089] Finally, the cells were cultured in a 37°C incubator for 24 h.

[0090] The blank group was treated in a similar manner as described above, except that sterile water was used instead of the MOF stock solution.

[0091] Figure 6 A photograph of a Staphylococcus aureus agar plate treated with a scandium metal organic framework solution in this example is shown. Figure 7 The figure shows the survival rate of Staphylococcus aureus after being treated with the scandium metal organic framework solution in this embodiment.

[0092] Figure 8 A photograph of an E. coli agar plate treated with a scandium metal organic framework solution in this example is shown. Fig. 9 The figure shows the survival rate of Escherichia coli after being treated with the scandium metal organic framework solution in this example.

[0093] As can be seen from the above figure, the use of scandium metal organic framework solution as a bactericide in photodynamic sterilization has a good killing effect on Staphylococcus aureus and Escherichia coli.

[0094] It can be seen from this example that Sc-TCPP MOF can achieve ultra-low dose (5 μg / mL) and low irradiance (12 mW / cm 2 ) and low illumination time (10 min), with a sterilization rate of more than 90%. The metal-organic framework of porphyrin synthesized by microplasma technology can significantly improve the bactericidal activity (the sterilization effect of 5 μg / mL metal-organic framework can reach 60% within 10 min without illumination).

[0095] Embodiment 3,

[0096] This example is used to illustrate the effect of the scandium metal organic framework on the photodynamic sterilization effect of Staphylococcus aureus under light of different wavelengths.

[0097] The scandium metal organic framework solution used in this example was prepared according to the steps described in Example 1, and the cultivation and killing steps of Staphylococcus aureus in this example were the same as those in Example 2. The difference was that the final concentration of the scandium metal organic framework solution for treating Staphylococcus aureus was 5 μg / mL, and the wavelength of the light used was different.

[0098] Specifically, during the irradiation process, the irradiation intensity was controlled to be the same at 12 mW / cm 2 The illumination time was 10 min, and the wavelengths of light were 420nm, 470nm, 570nm and 660nm respectively. The final results are as follows Fig.10 As shown, Fig.10 Figure 2 shows photos of a Staphylococcus aureus agar plate treated with a scandium metal organic framework solution at different wavelengths in this example. Fig.11 The bacterial survival rates of Staphylococcus aureus treated with the scandium metal organic framework solution at different wavelengths in this embodiment are shown. It can be seen from the figure that the irradiation with 420nm wavelength light has a good killing effect on Staphylococcus aureus.

[0099] It can be seen from this embodiment that the scandium metal organic framework material itself has a wide ultraviolet absorption in the visible light region, which can achieve a certain degree of inactivation of bacteria under multiple wavelengths of light, and still has a good bactericidal effect at a longer wavelength of 660 nm.

[0100] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a metal organic framework material, characterized in that: The preparation method comprises: Adding meso-tetrakis(4-carboxyphenyl)porphine into N,N-dimethylformamide for dissolution to prepare solution A; Scandium chloride hexahydrate is added into ultrapure water and dissolved to prepare a solution B; The prepared solution A and solution B were mixed, and ultrasonic treatment was performed to fully mix the two solutions to prepare a mixed solution, wherein the ultrasonic treatment time was 2 min, and the ultrasonic frequency was 40 kHz; The mixed solution is subjected to micro plasma treatment for 45 to 60 minutes; The mixed solution after the micro-plasma treatment is centrifuged to obtain a metal organic framework solid.

2. The method for preparing a metal organic framework material according to claim 1, characterized in that: The preparation method also includes washing and precipitating the metal organic framework solid, freeze-drying the precipitate in a vacuum freeze dryer, adding ultrapure water to the precipitate obtained after freeze drying to form a 0.5 mg / mL solution, and storing it in an environment of 0-4°C.

3. The method for preparing a metal organic framework material according to claim 2, characterized in that: The washing precipitate comprises washing the precipitate with dimethylformamide and ethanol for three times.

4. The method for preparing a metal organic framework material according to claim 1, characterized in that: The freeze-drying time is 12 to 24 hours.

5. The method for preparing a metal organic framework material according to claim 1, characterized in that: The micro plasma treatment comprises: A platinum electrode as an anode is completely immersed in the mixed solution; Place a hollow stainless steel tube 3-5 mm above the liquid surface of the mixed solution, and blow argon gas into the liquid surface from the bottom of the hollow stainless steel tube at a rate of 100 mL / min; Using a plasma discharge module, an input voltage of 7 V was applied to form a micro plasma between the mixed solution and the bottom of the stainless steel tube, and the discharge lasted for 45 to 60 minutes.

6. The method for preparing a metal organic framework material according to claim 1, characterized in that: The centrifugal treatment includes a centrifuge speed of 10000-12000 rpm and a centrifugal time of 20-30 min.

7. A metal organic framework material, characterized in that: The metal organic framework material is prepared according to the method according to any one of claims 1 to 5.

8. Application of a metal organic framework material in photodynamic sterilization, characterized in that: The metal organic framework material prepared by the method according to any one of claims 1 to 5 is used for photodynamic sterilization.

9. The use of the metal organic framework material in photodynamic sterilization according to claim 8, characterized in that: In the photodynamic sterilization, the added amount of the metal organic framework material is 5-20 μg / mL.

10. The use of the metal organic framework material in photodynamic sterilization according to claim 8, characterized in that: In the photodynamic sterilization, the wavelength of the irradiated light is 420-660 nm, and the irradiation intensity is 12 mW / cm 2 , the irradiation time is 10 min.

Citation Information

Patent Citations

  • Method for modifying MOFs material through low-temperature plasma and application of MOFs material

    CN113019329A

  • Method for improving photodynamic therapy efficiency of porphyrin metal organic framework by constructing heterojunction and application

    CN117180424A

  • Synthesis method of MOFs (Metal-Organic Frameworks) based on ligand guidance

    CN118307790A

  • Selective adsorption of carbon dioxide by a metal-organic framework

    WO2019202105A1