Environment-friendly water-based high-temperature-resistant paint as well as preparation method and application thereof
Through environmentally friendly water-based high-temperature resistant paint with components such as water-based silicone resin, the environmental protection and technical barriers of traditional solvent-based high-temperature resistant paint are solved, and a low VOC, energy-saving and environmentally friendly coating is achieved, with high density and excellent Heat resistance, suitable for aerospace and new energy vehicles.
Patent Information
- Application Number
- CN202411308189.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-19
AI Technical Summary
Traditional solvent-based high-temperature resistant paints have environmental protection problems and technical barriers, and are difficult to meet the requirements of environmental protection and international standards. Especially in the fields of aerospace and new energy vehicles, it is difficult to replace traditional paints.
Use water-based silicone resin, color paste, anti-deposition agent, anti-flash rust agent, epoxy phosphate, wetting agent, defoaming agent, thickening agent, glass powder, mica powder, copper chrome black and zinc phosphate. The environmentally friendly water-based high-temperature resistant paint is prepared through specific stirring and filtration steps to form a low VOC, energy-saving and environmentally friendly coating, with high density and excellent heat resistance.
The reaction between low-melting point glass powder and silicone resin is realized to form refractory substances, provide high temperature resistance, acid and alkali resistance, water resistance and excellent adhesion, improve the salt spray resistance, flexibility and gloss of the coating film, and is equipped with Extremely excellent hiding power and anti-rust performance, suitable for surface treatment of mechanical equipment.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to an environmentally friendly water-based high-temperature resistant paint and a preparation method and application thereof. Background Art
[0002] High temperature resistant paint is a special functional coating. Its coating maintains its performance and stability in high temperature environment to extend the service life of the equipment. It is widely used in aerospace, new energy vehicles, petroleum metallurgy, electrical equipment and other fields.
[0003] The policies implemented by the high temperature resistant industry restrict the expansion of backward production capacity, put forward requirements to improve product quality and technical level, encourage technological upgrading and promote green development, so traditional solvent-based high temperature resistant paint will gradually be replaced by environmentally friendly high temperature resistant paint.
[0004] With the development of aerospace technology, the upgrading of industrialization and the popularization of new energy vehicles, the demand for high temperature resistant paint is increasing. More importantly, the international standards of traditional solvent-based high temperature resistant paints have formed technical barriers, restricting the development of enterprises. Therefore, it is of great significance to develop environmentally friendly high temperature resistant paints to break through the technical barriers of international standards for high temperature resistance. Summary of the invention
[0005] The purpose of the present invention is to provide an environmentally friendly water-based high temperature resistant paint and a preparation method and application thereof, which can at least solve one of the above problems.
[0006] According to one aspect of the present invention, there is provided an environmentally friendly water-based high temperature resistant paint, comprising the following components in parts by weight:
[0007] Waterborne silicone resin, 65-68 parts;
[0008] Color paste, 25-30 parts;
[0009] Anti-settling agent A, 2-3 parts;
[0010] Anti-flash rust agent, 0.5-1 part;
[0011] Epoxy phosphate, 0.6-1 part;
[0012] Wetting agent, 0.1-0.3 parts;
[0013] Defoamer A, 0.1-0.3 parts;
[0014] Thickener, 1-2 parts;
[0015] The color paste includes the following components in parts by weight:
[0016] Dispersant, 1-2 parts;
[0017] Rheological additive, 1-2 parts;
[0018] Anti-settling agent B, 0.1-2 parts;
[0019] Defoamer B, 0.1-0.5 parts;
[0020] Glass powder, 18-22 parts;
[0021] Mica powder, 5-10 parts;
[0022] Copper chrome black, 15-18 parts;
[0023] Zinc phosphate, 8-10 parts;
[0024] The balance is water.
[0025] In some embodiments, the water-based silicone resin is 67 parts, the color paste is 26-29 parts, the anti-settling agent A is 2.7 parts, the anti-flash rust agent is 0.6-1 part, the epoxy phosphate is 0.6-1 part, the wetting agent is 0.2 part, the defoamer A is 0.1 part, and the thickener is 1.3 parts.
[0026] In some embodiments, the color paste is 27.5 parts, the anti-flash rust agent is 0.6 parts, and the epoxy phosphate is 0.6 parts.
[0027] In some embodiments, the color paste includes the following components in parts by weight:
[0028] Water, 43.8 parts;
[0029] Dispersant, 2 parts;
[0030] Rheological additive, 1.5 parts;
[0031] Anti-settling agent B, 0.2 part;
[0032] Defoamer B, 0.2 part;
[0033] Glass powder, 20 parts;
[0034] Mica powder, 8 parts;
[0035] Copper chrome black, 16 parts;
[0036] Zinc phosphate, 8.3 parts.
[0037] In some embodiments, the glass powder is 350° C. melt glass powder.
[0038] In some embodiments, the water is deionized water.
[0039] According to another aspect of the present invention, a method for preparing an environmentally friendly water-based high temperature resistant paint is provided, characterized in that it comprises at least the following steps:
[0040] S1. Preparation of color paste:
[0041] First, add water, dispersant, rheological additive, anti-settling agent B and defoamer into the stirring device in order, stir for 5 minutes, then add glass powder, mica powder, copper chrome black and zinc phosphate, stir for another 45 minutes, and set aside;
[0042] S2. Preparation of environmentally friendly water-based high temperature resistant paint:
[0043] Add water-based silicone resin, the color paste prepared in step S1, anti-settling agent A, anti-flash rust agent, epoxy phosphate, wetting agent, defoaming agent A and thickener into a stirring device in sequence, disperse and stir evenly, adjust the viscosity to 80Ku, and then filter through a 200-mesh filter to obtain an environmentally friendly water-based high-temperature resistant paint.
[0044] In some embodiments, in step S1, the speed of the stirring device is first controlled at 1000 r / min, and then water, dispersant, rheological additive, anti-settling agent B and defoaming agent B are added to the stirring device in sequence. After stirring for 5 minutes, the speed of the stirring device is controlled at 1500 r / min, and then glass powder, mica powder, copper chrome black and zinc phosphate are added, and then stirred for 45 minutes.
[0045] In some embodiments, in step S2, the rotation speed of the stirring device is controlled at 1500 r / min, and the stirring time is 30 min.
[0046] According to another aspect of the present invention, an application of an environmentally friendly water-based high temperature resistant paint is also provided, characterized in that the environmentally friendly water-based high temperature resistant paint prepared by the above-mentioned preparation method of the environmentally friendly water-based high temperature resistant paint is suitable for surface treatment of mechanical equipment, and the specific application method comprises the following steps:
[0047] A. Before spraying, remove oil and rust from the equipment surface;
[0048] B. Spray environmentally friendly water-based high-temperature resistant paint on the surface of the equipment by spraying, and the paint film thickness is controlled at 35-50μm;
[0049] C. Bake at 200-280℃ for 15-60min to cure.
[0050] Beneficial effects of the present invention:
[0051] The invention provides a low-VOC, energy-saving, environmentally friendly, and safe-to-construct water-based system high-temperature-resistant and anti-corrosion coating. The environmentally friendly water-based high-temperature-resistant paint forms a refractory substance by reacting low-melting-point glass powder with an organic silicone resin at 350°C to isolate oxygen, thereby forming a high-density glass coating that is resistant to high temperatures, yellowing, acid and alkali in the resin paint; the main function of epoxy phosphate is to improve the adhesion of the coating to the metal surface, improve the water resistance, salt spray resistance and flexibility of the coating film, and improve the gloss and hardness; the role of mica powder in water-based organic silicone resin paint mainly includes barrier effect, improvement of the physical and mechanical properties of the paint film, improvement of the wear resistance of the paint film, provision of insulation performance, flame retardancy, UV resistance and infrared characteristics, as well as sound insulation and shock absorption; copper chrome black plays a key role in water-based organic silicone resin paint, which is mainly manifested in its excellent heat resistance, light resistance, chemical resistance and extremely excellent hiding power; the role of zinc phosphate in the color paste is mainly as an anti-rust pigment, providing excellent anti-rust performance and water resistance. After testing, it is found that it not only has strong adhesion, but also has excellent properties such as resistance to high temperature, resistance to sudden cold, and resistance to smoke. DETAILED DESCRIPTION
[0052] The present invention is further described in detail below.
[0053] The environmentally friendly water-based high temperature resistant paint of the present invention comprises the following components in parts by weight:
[0054] Waterborne silicone resin, 65-68 parts;
[0055] Color paste, 25-30 parts;
[0056] Anti-settling agent A, 2-3 parts;
[0057] Anti-flash rust agent, 0.5-1 part;
[0058] Epoxy phosphate, 0.6-1 part;
[0059] Wetting agent, 0.1-0.3 parts;
[0060] Defoamer A, 0.1-0.3 parts;
[0061] Thickener, 1-2 parts;
[0062] The color paste includes the following components in parts by weight:
[0063] Dispersant, 1-2 parts;
[0064] Rheological additive, 1-2 parts;
[0065] Anti-settling agent B, 0.1-2 parts;
[0066] Defoamer B, 0.1-0.5 parts;
[0067] Glass powder, 18-22 parts;
[0068] Mica powder, 5-10 parts;
[0069] Copper chrome black, 15-18 parts;
[0070] Zinc phosphate, 8-10 parts;
[0071] The balance is water.
[0072] Preferably, the water-based silicone resin is 67 parts, the color paste is 26-29 parts, the anti-settling agent A is 2.7 parts, the anti-flash rust agent is 0.6-1 part, the epoxy phosphate is 0.6-1 part, the wetting agent is 0.2 part, the defoaming agent A is 0.1 part, and the thickener is 1.3 parts.
[0073] More preferably, the color paste is 27-28 parts, the anti-flash rust agent is 0.6 parts, and the epoxy phosphate is 0.6 parts.
[0074] Preferably, the glass powder is 350°C molten glass powder.
[0075] Preferably, the water is deionized water.
[0076] Preferably, the water-based silicone resin uses FNMT3003 water-based silicone resin manufactured by Zhangjiagang Noto Chemical Technology Co., Ltd.; the anti-settling agent A and the anti-settling agent B are the same, both using BENTONE LT water-based rheological additive produced by Hemingside, which is a rheological additive made of modified montmorillonite clay; the anti-flash rust agent uses Tech-8387 anti-flash rust agent produced by Shanghai Tiger Polymer Technology Co., Ltd.; the wetting agent uses Dego substrate wetting agent Twin 4100; the defoamer A is BYK024 defoamer produced by BYK; the thickener uses Hemingside DeuRheo WT-105A water-based paint thickener; the dispersant is BYK190 dispersant produced by BYK; and the rheological additive is BYK420 rheological agent produced by BYK.
[0077] The invention provides a low-VOC, energy-saving, environmentally friendly, and safe-to-construct water-based system high-temperature-resistant and anti-corrosion coating. The environmentally friendly water-based high-temperature-resistant paint forms a refractory substance by reacting low-melting-point glass powder with an organic silicone resin at 350°C to isolate oxygen, thereby forming a high-density glass coating that is resistant to high temperatures, yellowing, acid and alkali in the resin paint; the main function of epoxy phosphate is to improve the adhesion of the coating to the metal surface, improve the water resistance, salt spray resistance and flexibility of the coating film, and improve the gloss and hardness; the role of mica powder in water-based organic silicone resin paint mainly includes barrier effect, improvement of the physical and mechanical properties of the paint film, improvement of the wear resistance of the paint film, provision of insulation performance, flame retardancy, UV resistance and infrared characteristics, as well as sound insulation and shock absorption; copper chrome black plays a key role in water-based organic silicone resin paint, which is mainly manifested in its excellent heat resistance, light resistance, chemical resistance and extremely excellent hiding power; the role of zinc phosphate in the color paste is mainly as an anti-rust pigment, providing excellent anti-rust performance and water resistance. After testing, it is found that it not only has strong adhesion, but also has excellent properties such as resistance to high temperature, resistance to sudden cold, and resistance to smoke.
[0078] The present invention also discloses a method for preparing the above-mentioned environmentally friendly water-based high temperature resistant paint, which at least comprises the following steps:
[0079] S1. Preparation of color paste:
[0080] First, add water, dispersant, rheological additive, anti-settling agent B and defoamer B into the stirring device in order, stir for 5 minutes, then add glass powder, mica powder, copper chrome black and zinc phosphate, stir for another 45 minutes, and set aside;
[0081] S2. Preparation of environmentally friendly water-based high temperature resistant paint:
[0082] Add water-based silicone resin, the color paste prepared in step S1, anti-settling agent A, anti-flash rust agent, epoxy phosphate, wetting agent, defoaming agent A and thickener into a stirring device in sequence, disperse and stir evenly, adjust the viscosity to 80Ku, and then filter through a 200-mesh filter to obtain an environmentally friendly water-based high-temperature resistant paint.
[0083] In some embodiments, in step S1, the speed of the stirring device is first controlled at 1000 r / min, and then water, dispersant, rheological additive, anti-settling agent B and defoaming agent B are added to the stirring device in sequence. After stirring for 5 minutes, the speed of the stirring device is controlled at 1500 r / min, and then glass powder, mica powder, copper chrome black and zinc phosphate are added, and then stirred for 45 minutes.
[0084] In some embodiments, in step S2, the rotation speed of the stirring device is controlled at 1500 r / min, and the stirring time is 30 min.
[0085] The present invention also discloses an application of an environmentally friendly water-based high temperature resistant paint prepared by the above-mentioned preparation method of the environmentally friendly water-based high temperature resistant paint. The environmentally friendly water-based high temperature resistant paint is suitable for surface treatment of mechanical equipment. The specific application method comprises the following steps:
[0086] A. Before spraying, remove oil and rust from the equipment surface;
[0087] B. Spray environmentally friendly water-based high-temperature resistant paint on the surface of the equipment by spraying, and the paint film thickness is controlled at 35-50μm;
[0088] C. Bake at 200-280℃ for 15-60min to cure.
[0089] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0090] Example 1
[0091] This embodiment provides an environmentally friendly water-based high temperature resistant paint. The specific components and proportions of the environmentally friendly water-based high temperature resistant paint are shown in the following Table 1:
[0092] Table 1: Proportion table of environmentally friendly water-based high temperature resistant paint of Example 1
[0093] Components Weight Waterborne silicone resin 67 Color paste 27.5 Anti-settling agent A 2.7 Anti-flash rust agent 0.6 Epoxy Phosphate 0.6 Wetting Agents 0.2 Defoamer A 0.1 Thickener 1.3
[0094] The specific components and proportions of the color paste in the above-mentioned environmentally friendly water-based high temperature resistant paint are shown in Table 2 below:
[0095] Table 2: Proportion table of the color paste of Example 1
[0096] Components Weight Dispersants 2 Rheology additives 1.5 Anti-settling agent B 0.2 Defoamer B 0.2 Glass powder 20 Mica powder 8 Copper Chrome Black 16 Zinc phosphate 8.3 water 43.8
[0097] According to the ratio table in Table 1-2 above, the above environmentally friendly water-based high temperature resistant paint is prepared by the following preparation method, which specifically includes the following steps:
[0098] S1. Preparation of color paste:
[0099] First control the speed of the stirring equipment at 1000r / mm i nThen, add 43.8 parts of water, 2 parts of dispersant, 1.5 parts of rheological additive, 0.2 parts of anti-settling agent B and 0.2 parts of defoaming agent B into the stirring device in turn. After stirring for 5min, control the speed of the stirring device at 1500r / mmin, add 20 parts of glass powder, 8 parts of mica powder, 16 parts of copper chrome black and 8.3 parts of zinc phosphate, and stir for another 45min for standby use; check whether there is precipitation and whether there is any abnormality.
[0100] S2. Preparation of environmentally friendly water-based high temperature resistant paint:
[0101] Add 67 parts of water-based silicone resin, 27.5 parts of the color paste prepared in step S1, 2.7 parts of anti-settling agent A, 0.6 parts of anti-flash rust agent, 0.6 parts of epoxy phosphate, 0.2 parts of wetting agent, 0.1 parts of defoamer A and 1.3 parts of thickener in a stirring device in sequence, disperse and stir evenly, and adjust the viscosity to 80K u , and then filtered through a 200-mesh filter to obtain an environmentally friendly water-based high-temperature resistant paint.
[0102] Example 2
[0103] This embodiment provides another environmentally friendly water-based high temperature resistant paint. The specific components and proportions of the environmentally friendly water-based high temperature resistant paint are shown in Table 3 below:
[0104] Table 3: Proportion table of environmentally friendly water-based high temperature resistant paint of Example 2
[0105] Components Weight Waterborne silicone resin 67 Color paste 28 Anti-settling agent A 2.2 Anti-flash rust agent 0.6 Epoxy Phosphate 0.6 Wetting Agents 0.2 Defoamer A 0.1 Thickener 1.3
[0106] The specific components and proportions of the color paste in the above-mentioned environmentally friendly water-based high temperature resistant paint are shown in Table 4 below:
[0107] Table 4: Proportion table of the color paste of Example 2
[0108] Components Weight Dispersants 2 Rheology additives 1.5 Anti-settling agent B 0.2 Defoamer B 0.2 Glass powder 21 Mica powder 7.3 Copper Chrome Black 15 Zinc phosphate 9 water 43.8
[0109] According to the ratio table in Table 3-4 above, the above environmentally friendly water-based high temperature resistant paint is prepared by the following preparation method, which specifically includes the following steps:
[0110] S1. Preparation of color paste:
[0111] First, control the speed of the stirring equipment at 1000r / min, and then add 43.8 parts of water, 2 parts of dispersant, 1.5 parts of rheological additive, 0.2 parts of anti-settling agent B and 0.2 parts of defoaming agent B into the stirring equipment in sequence. After stirring for 5 minutes, control the speed of the stirring equipment at 1500r / min, add 21 parts of glass powder, 7.3 parts of mica powder, 15 parts of copper chrome black and 9 parts of zinc phosphate, and stir for another 45 minutes for use; check whether there is precipitation and whether there is any abnormality.
[0112] S2. Preparation of environmentally friendly water-based high temperature resistant paint:
[0113] 67 parts of water-based silicone resin, 28 parts of the color paste prepared in step S1, 2.2 parts of anti-settling agent A, 0.6 parts of anti-flash rust agent, 0.6 parts of epoxy phosphate, 0.2 parts of wetting agent, 0.1 parts of defoaming agent A and 1.3 parts of thickener are added in sequence to a stirring device, dispersed and stirred evenly, the viscosity is adjusted to 80Ku, and then filtered through a 200-mesh filter to obtain an environmentally friendly water-based high-temperature resistant paint.
[0114] Example 3
[0115] The environmentally friendly water-based high temperature resistant paint prepared in the above-mentioned Examples 1 and 2 is coated on a test metal plate (test plate) according to the above-mentioned application method, and the performance of the environmentally friendly water-based high temperature resistant paint prepared in the above-mentioned Examples 1 and 2 is tested using the known national standard method. Specifically, the test items include curing conditions, state in the container, anti-decarburization, cross-cutting test, heat resistance, salt spray resistance, sudden cooling resistance, coating peeling performance, etc., and the specific test standards and test methods are shown in Table 5 below:
[0116] Table 5: Test items and their test standards or test methods
[0117]
[0118] According to the test standards and test methods in Table 5, the performance test results of the environmentally friendly water-based high temperature resistant paint of Example 1 and Example 2 are obtained and refer to the following Table 6:
[0119] Table 6: Performance test table of environmentally friendly water-based high temperature resistant paint of Example 1 and Example 2
[0120]
[0121] According to the above data, the environmentally friendly water-based high temperature resistant paint of the present invention not only has the advantages of good anti-decarburization performance and good adhesion effect, but also has excellent properties such as heat resistance, salt spray resistance and sudden cooling resistance.
[0122] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. An environmentally friendly water-based high temperature resistant paint, characterized in that: The invention comprises the following components in parts by weight: Waterborne silicone resin, 65-68 parts; Color paste, 25-30 parts; Anti-settling agent A, 2-3 parts; Anti-flash rust agent, 0.5-1 part; Epoxy phosphate, 0.6-1 part; Wetting agent, 0.1-0.3 parts; Defoamer A, 0.1-0.3 parts; Thickener, 1-2 parts; The color paste includes the following components by weight: Dispersant, 1-2 parts; Rheological additive, 1-2 parts; Anti-settling agent B, 0.1-2 parts; Defoamer B, 0.1-0.5 parts; Glass powder, 18-22 parts; Mica powder, 5-10 parts; Copper chrome black, 15-18 parts; Zinc phosphate, 8-10 parts; The balance is water.
2. The environmentally friendly water-based high temperature resistant paint according to claim 1, characterized in that: The water-based silicone resin is 67 parts, the color paste is 26-29 parts, the anti-settling agent A is 2.7 parts, the anti-flash rust agent is 0.6-1 part, the epoxy phosphate is 0.6-1 part, the wetting agent is 0.2 part, the defoaming agent A is 0.1 part, and the thickener is 1.3 parts.
3. The environmentally friendly water-based high temperature resistant paint according to claim 2, characterized in that: The color paste is 27.5 parts, the anti-flash rust agent is 0.6 parts, and the epoxy phosphate is 0.6 parts.
4. The environmentally friendly water-based high temperature resistant paint according to claim 1, characterized in that: The color paste includes the following components by weight: Water, 43.8 parts; Dispersant, 2 parts; Rheological additive, 1.5 parts; Anti-settling agent B, 0.2 part; Defoamer B, 0.2 part; Glass powder, 20 parts; Mica powder, 8 parts; Copper chrome black, 16 parts; Zinc phosphate, 8.3 parts.
5. The environmentally friendly water-based high temperature resistant paint according to claim 1, characterized in that: The glass powder is 350° C. molten glass powder.
6. The environmentally friendly water-based high temperature resistant paint according to claim 1, characterized in that: The water is deionized water.
7. A method for preparing an environmentally friendly water-based high temperature resistant paint, characterized in that: At least the following steps are included: S1. Preparation of color paste: First, add water, dispersant, rheological additive, anti-settling agent B and defoamer into the stirring device in order, stir for 5 minutes, then add glass powder, mica powder, copper chrome black and zinc phosphate, stir for another 45 minutes, and set aside; S2. Preparation of environmentally friendly water-based high temperature resistant paint: Add water-based silicone resin, the color paste prepared in step S1, anti-settling agent A, anti-flash rust agent, epoxy phosphate, wetting agent, defoaming agent A and thickener into a stirring device in sequence, disperse and stir evenly, adjust the viscosity to 80Ku, and then filter through a 200-mesh filter to obtain an environmentally friendly water-based high-temperature resistant paint.
8. The method for preparing the environmentally friendly water-based high temperature resistant paint according to claim 7, characterized in that: In step S1, the speed of the stirring device is first controlled at 1000 r / min, and then water, dispersant, rheological additive, anti-settling agent B and defoaming agent B are added to the stirring device in sequence. After stirring for 5 minutes, the speed of the stirring device is controlled at 1500 r / min, and then glass powder, mica powder, copper chrome black and zinc phosphate are added, and then stirred for another 45 minutes.
9. The method for preparing the environmentally friendly water-based high temperature resistant paint according to claim 7, characterized in that: In step S2, the rotation speed of the stirring device is controlled at 1500 r / min, and the stirring time is 30 min.
10. An application of an environmentally friendly water-based high temperature resistant paint, characterized in that: The environmentally friendly water-based high-temperature resistant paint prepared by the preparation method of the environmentally friendly water-based high-temperature resistant paint according to any one of claims 7 to 9 is suitable for surface treatment of mechanical equipment, and the specific application method comprises the following steps: A. Before spraying, remove oil and rust from the equipment surface; B. Spray environmentally friendly water-based high-temperature resistant paint on the surface of the equipment by spraying, and the paint film thickness is controlled at 35-50μm; C. Bake at 200-280℃ for 15-60min to cure.
Citation Information
Patent Citations
Water-based organic silicon anticorrosive paint and preparation method thereof
CN113861838A
Environment-friendly high-temperature-resistant insulating paint and preparation method thereof
CN116042086A
Water-based heavy anti-corrosion coating and preparation method thereof
CN117384527A
Cited By
Water-based environment-friendly coating with high-temperature resistance, corrosion resistance and high-temperature discoloration resistance as well as preparation method and application of water-based environment-friendly coating