Preparation method of sludge-based magnetic biomass charcoal

By cleaning the remaining sludge in the sewage treatment plant and high-temperature carbonization treatment, magnetic biomass charcoal was prepared, which solved the problems of secondary pollution and insufficient resource utilization in sludge treatment, and achieved efficient and environmentally friendly sludge resource utilization Treatment reduces environmental impact and costs.

CN118976464APending Publication Date: 2024-11-19DONGHUA UNIV

Patent Information

Application Number
CN202411087510.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art has problems such as secondary pollution, high cost, environmental hazards and insufficient resource utilization when treating sludge. Especially when using sludge to prepare magnetic biomass charcoal, it lacks efficient and environmentally friendly methods.

Method used

By cleaning and high-temperature carbonization of the remaining sludge retrieved from the sewage treatment plant, carbonizing in a nitrogen atmosphere with a tube furnace, controlling the temperature and time, biomass carbon with magnetic properties is prepared to avoid the addition of iron and reduce the amount of iron. Cost and environmental impact.

Benefits of technology

The harmless, resource-based and reduced sludge treatment has been achieved, the utilization rate of sludge has been improved, environmental pollution has been reduced, and the preparation process is simple and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976464A_ABST
    Figure CN118976464A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of sludge-based magnetic biomass charcoal, which comprises the following steps: (1) cleaning residual sludge obtained by a sewage treatment plant with clear water for 2-3 times, then putting the residual sludge into an air dry oven for drying and dewatering, and carrying out pretreatment; and (2) carrying out high-temperature firing on the pretreated sludge by using a tubular furnace to obtain the magnetic biomass charcoal. The prepared magnetic biomass charcoal is found to have high capacitance and excellent conductivity, and when the magnetic biomass charcoal is put into an anaerobic digestion system, the degradation efficiency of organic matters and the production efficiency of methane can be effectively improved. Besides, according to the prepared sludge-based magnetic biomass charcoal, the existing treatment method of the residual sludge is improved, secondary pollution and other harms are avoided, the residual sludge is more effectively utilized, and recycling, harmlessness and reduction of the residual sludge are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of resource disposal and utilization of surplus sludge, and specifically relates to a method for preparing sludge-based magnetic biochar by utilizing surplus sludge from a sewage treatment plant. Background Art

[0002] As a byproduct of sewage treatment, residual sludge has the characteristics of large volume, high water content and complex composition. Traditional sludge treatment and disposal methods: (1) Agricultural utilization: After the residual sludge is treated by stabilization technology, because its product contains a large amount of nutrients such as N, P, K and organic matter, it can be used as agricultural fertilizer or as a soil conditioner in the soil, thereby reducing its secondary pollution and achieving effective utilization and management. However, there are also toxic and harmful substances in the product, such as heavy metals, which need further treatment, so the promotion of this technology is limited. (2) Sanitary landfill: This method is simple to operate, economically feasible, and the landfilled residual sludge can be gradually degraded over time. However, this practice occupies a large amount of land and causes harmful substances to infiltrate and pollute groundwater. This sludge disposal technology method can only be used as an emergency measure and does not achieve the purpose of truly treating residual sludge. (3) Sludge incineration: Sludge incineration is simple to operate, can greatly reduce the amount of residual sludge, and can recover energy in the process. It has become a more commonly used disposal method at the current stage. However, due to the high water content of the residual sludge, a large amount of energy will be consumed during the incineration process, resulting in high costs. In addition, carcinogens such as dioxins will be produced during the combustion process, which will seriously harm the environment.

[0003] Residual sludge contains rich organic matter and has great potential for resource utilization. It is worth noting that iron salts may be added in sewage and wastewater coagulation treatment, chemical phosphorus removal and sludge dehydration units, resulting in the sludge often containing a large amount of iron, which provides conditions for the direct use of sludge to prepare magnetic biochar. Therefore, the use of iron-containing residual sludge to prepare an environmentally friendly conductive material, magnetic biochar, to improve the efficiency of anaerobic biological treatment systems can solve the problem of high prices of commonly used conductive materials and improve the economic feasibility of using conductive materials to strengthen anaerobic processes. In addition, this method solves the problem of the final disposal of residual sludge, thereby achieving efficient resource utilization of these sludges.

[0004] In general, the preparation of sludge-based biochar focuses more on carbonization and the adsorption characteristics of biochar; while sludge-based magnetic biochar focuses more on the content and form of iron in the sludge. Therefore, the form of the preparation reactor, the control of the iron element in the preparation raw materials, and the control of the temperature and oxygen content of the preparation process are crucial. Summary of the invention

[0005] The present invention aims at optimizing and improving the existing technology for the treatment of excess sludge, in order to better utilize the excess sludge materials as resources, and effectively utilize the excess sludge to prepare magnetic biomass charcoal, avoiding the secondary pollution and defects of the existing excess sludge disposal, and realizing the harmless, resource-based, and reduced-volume treatment of the excess sludge. The present invention provides a resource-based treatment method for the excess sludge from a sewage treatment plant.

[0006] The specific steps of the preparation method of a sludge-based magnetic biochar provided by the present invention are as follows:

[0007] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0008] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to burn it. The burning conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 400-800°C for carbonization. After a fixed carbonization time, naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0009] (3) Preparing a finished sludge-based magnetic biochar product: Grinding the crude sludge-based magnetic biochar product obtained in step (2) into powder to obtain a finished magnetic biochar product.

[0010] Furthermore, the raw material in step (1) is residual sludge obtained from a sewage treatment plant, and step (1) also includes measuring the iron content and pH value of the cleaned sludge material. The iron content in the cleaned solution is not less than 10%, and the pH value is 6-8.

[0011] Furthermore, when the iron content in the cleaned sludge material is lower than 10%, a certain amount of iron salt is added to the sludge material, and the iron salt is one or more of ferric chloride, ferrous sulfate, and ferrous chloride. When the pH value of the cleaned sludge material is lower than 6, a certain amount of ammonia water is added to the sludge material. When the pH value of the cleaned sludge material is higher than 8, a certain amount of hydrochloric acid solution is added to the sludge material.

[0012] Furthermore, in the step (1), the cleaned sludge material is allowed to settle for 30 minutes, and after confirming that the upper clear liquid is free of suspended matter, it is transferred to a blast drying oven for dehydration treatment. The moisture content of the biomass charcoal raw material obtained after drying shall not be higher than 5%.

[0013] Furthermore, in step (2), the carbonization time after the tubular furnace is heated is 30 minutes.

[0014] Furthermore, the magnetic biochar product obtained in step (3) has a powder particle size of less than 5 microns.

[0015] The present invention has the following beneficial effects:

[0016] 1. The method of the present invention adopts high-temperature carbonization in a tubular furnace to prepare the material. The carbonization process is in a nitrogen atmosphere, thereby avoiding the loss of biochar.

[0017] 2. The method of the present invention utilizes the residual sludge generated by the sewage treatment plant as raw material, avoiding the shortcomings of secondary pollution caused by the original residual sludge disposal method, causing less pollution to the environment, greatly improving the utilization rate of the residual sludge, alleviating the pollution problem of the residual sludge, and realizing true resource utilization, harmlessness, and reduction.

[0018] 3. The present invention directly utilizes the residual sludge as raw material, and there is no need to add iron to the raw material in the subsequent operation process. The cost is low, the preparation process is simple, and it is convenient for engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0020] Figure 1 Design a process diagram of the sludge-based magnetic biochar preparation system for the present invention;

[0021] Figure 2 This is a low-magnification scanning electron microscope (SEM) image of an embodiment of sludge-based magnetic biochar;

[0022] Figure 3 This is a high-magnification scanning electron microscope (SEM) image of an embodiment of sludge-based magnetic biochar;

[0023] Figure 4 It is the Fourier infrared FTIR spectrum of the sludge-based magnetic biochar embodiment;

[0024] Figure 5 It is the XRD analysis characterization spectrum of the sludge-based magnetic biochar embodiment;

[0025] Figure 6 The degradation effect of the sludge-based magnetic biochar prepared by the present invention in the anaerobic biological treatment of COD in domestic wastewater;

[0026] Figure 7 The invention discloses the methane production and methane yield of the sludge-based magnetic biomass charcoal prepared by the present invention when applied to anaerobic biological treatment of domestic wastewater. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] A method for preparing sludge-based magnetic biochar comprises the following steps:

[0029] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0030] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to burn it. The burning conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 400-800°C for carbonization. After a fixed carbonization time, naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0031] (3) Preparing a finished sludge-based magnetic biochar product: Grinding the crude sludge-based magnetic biochar product obtained in step (2) into powder to obtain a finished magnetic biochar product.

[0032] The raw material in step (1) is the residual sludge obtained from the sewage treatment plant. Step (1) also includes measuring the iron content and pH value of the cleaned sludge material. The iron content in the cleaned solution is not less than 10%, and the pH value is 6-8.

[0033] Among them, when the iron content in the cleaned sludge material is lower than 10%, a certain amount of iron salt is added to the sludge material, and the iron salt is one or more of ferric chloride, ferrous sulfate, and ferrous chloride. When the pH value of the cleaned sludge material is lower than 6, a certain amount of ammonia water is added to the sludge material. When the pH value of the cleaned sludge material is higher than 8, a certain amount of hydrochloric acid solution is added to the sludge material.

[0034] Among them, in step (1), the cleaned sludge material is allowed to settle for 30 minutes, and after confirming that the upper clear liquid has no suspended matter, it is transferred to a blast drying oven for dehydration treatment. The moisture content of the biomass charcoal raw material obtained after drying shall not be higher than 5%.

[0035] Wherein, the carbonization time after the tubular furnace is heated in step (2) is 30 minutes.

[0036] The magnetic biochar product obtained in step (3) has a powder particle size of less than 5 microns.

[0037] Embodiment 1:

[0038] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0039] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to sinter it. The sintering conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 400°C for carbonization. The carbonization time is 30 minutes, and then naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0040] (3) Preparation of sludge-based magnetic biochar finished product: Grind the sludge-based magnetic biochar crude product obtained in step (2) into powder to obtain a sludge-based magnetic biochar finished product, which is abbreviated as B-400.

[0041] Embodiment 2:

[0042] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0043] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to sinter it. The sintering conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 500°C for carbonization. The carbonization time is 30 minutes, and then naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0044] (3) Preparation of sludge-based magnetic biochar finished product: Grind the sludge-based magnetic biochar crude product obtained in step (2) into powder to obtain a sludge-based magnetic biochar finished product, which is abbreviated as B-500.

[0045] Embodiment 3:

[0046] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0047] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to sinter it. The sintering conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 600°C for carbonization. The carbonization time is 30 minutes, and then naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0048] (3) Preparation of sludge-based magnetic biochar finished product: Grind the sludge-based magnetic biochar crude product obtained in step (2) into powder to obtain a sludge-based magnetic biochar finished product, which is abbreviated as B-600.

[0049] Embodiment 4:

[0050] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0051] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to sinter it. The sintering conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 700°C for carbonization. The carbonization time is 30 minutes, and then naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0052] (3) Preparation of sludge-based magnetic biochar finished product: Grind the sludge-based magnetic biochar crude product obtained in step (2) into powder to obtain a sludge-based magnetic biochar finished product, which is abbreviated as B-700.

[0053] Embodiment 5:

[0054] (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 2-3 times with clean water, and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours.

[0055] (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to sinter it. The sintering conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 800°C for carbonization. The carbonization time is 30 minutes, and then naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product.

[0056] (3) Preparation of sludge-based magnetic biochar finished product: Grind the sludge-based magnetic biochar crude product obtained in step (2) into powder to obtain a sludge-based magnetic biochar finished product, which is abbreviated as B-800.

[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0058] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing sludge-based magnetic biochar, It is characterized in that The steps include: (1) Pretreatment of sludge-based magnetic biochar raw materials: The residual sludge material retrieved from the sewage treatment plant was washed 23 times with clean water and then placed in a forced air drying oven at 105°C for drying and dehydration for 24 hours. (2) High-temperature carbonization process: Take an appropriate amount of pretreated sludge into a quartz boat and then use a tubular furnace to burn it. The burning conditions are: under nitrogen protection, continue to heat at a heating rate of 5°C / min to reach 400-800°C for carbonization. After a fixed carbonization time, naturally cool to room temperature to obtain a sludge-based magnetic biomass charcoal crude product. (3) Preparing a finished sludge-based magnetic biochar product: Grinding the crude sludge-based magnetic biochar product obtained in step (2) into powder to obtain a finished magnetic biochar product.

2. The method for preparing sludge-based magnetic biochar according to claim 1, It is characterized in that The raw material in step (1) is the residual sludge obtained from the sewage treatment plant. Step (1) also includes measuring the iron content and pH value of the cleaned sludge material. The iron content in the cleaned solution is not less than 10%, and the pH value is 6-8.

3. The method for preparing sludge-based magnetic biochar according to claim 2, It is characterized in that When the iron content in the cleaned sludge material is lower than 10%, a certain amount of iron salt is added to the sludge material, and the iron salt is one or more of ferric chloride, ferrous sulfate, and ferrous chloride. When the pH value of the cleaned sludge material is lower than 6, a certain amount of ammonia water is added to the sludge material. When the pH value of the cleaned sludge material is higher than 8, a certain amount of hydrochloric acid solution is added to the sludge material.

4. The method for preparing sludge-based magnetic biochar according to claim 1, It is characterized in that In the step (1), the cleaned sludge material is allowed to settle for 30 minutes, and after confirming that the upper clear liquid is free of suspended matter, it is transferred to a blast drying oven for dehydration treatment. The moisture content of the biomass charcoal raw material obtained after drying shall not be higher than 5%.

5. The method for preparing sludge-based magnetic biochar according to claim 1, It is characterized in that The carbonization time after the tubular furnace is heated in step (2) is 30 minutes.

6. The method for preparing sludge-based magnetic biochar according to claim 1, It is characterized in that The magnetic biochar product obtained in step (3) has a powder particle size of less than 5 microns.

Citation Information

Patent Citations

  • Method for enhancing printing and dyeing wastewater treatment efficiency by magnetic biological carbon

    CN108892312A

  • Sludge recycling method based on biochar firing and application of sludge recycling method

    CN110683729A

  • Modified biomass charcoal catalyst based on activated sludge and preparation method thereof

    CN111495349A

  • Preparation method of iron-containing sludge-based biochar material and application of same in anaerobic digestion

    CN111876173A

Cited By

  • Method for preparing activated carbon from mariculture bottom mud doped with biomass and application of activated carbon

    CN119774603A

  • Method for carrying out anaerobic digestion to recover phosphorus by adding sludge-based biochar

    CN120841802A