Antibacterial resin mixture, preparation method and application thereof, resin-permeable ceramic composite material and preparation method of resin-permeable ceramic composite material
By using an antibacterial resin mixture combining isothiazolinone compounds and acrylate monomers, resin-infiltrated ceramic composite materials were prepared by vacuum infiltration, which solved the problems of susceptibility to pathogenic bacteria infection and fracture, improved antibacterial and mechanical properties, and extended service life.
Patent Information
- Application Number
- CN202411038365.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Existing resin-infiltrated ceramic composite materials are susceptible to infection by pathogenic bacteria in the oral environment and have low fracture load, leading to repair failure and short service life.
An antibacterial resin mixture was prepared by combining isothiazolinone compounds as antibacterial agents with acrylate monomers through a vacuum infiltration method, forming a resin-infiltrated ceramic composite material that enhances antibacterial ability and mechanical properties.
It improves the antibacterial properties and fracture load of resin-infiltrated ceramic composites, reduces material fracture and secondary caries, and extends the service life of restorations.
Smart Images

Figure BDA0004973547380000091 
Figure BDA0004973547380000092 
Figure BDA0004973547380000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dental materials, and in particular to an antibacterial resin mixture and a preparation method and application thereof, a resin-infiltrated ceramic composite material and a preparation method thereof. Background Art
[0002] Dental caries is one of the most common chronic diseases in the human oral cavity. It is mainly caused by the acidic environment in the oral cavity caused by human daily eating habits, which gradually corrodes the tooth tissue. The main effective means of treating dental caries is filling and restorative materials. Dental resins and ceramic materials have become important materials for oral restorations due to their excellent safety, aesthetics and physical and chemical properties. However, resin or ceramic restorations generally experience material breakage, secondary caries and other phenomena during use, resulting in restoration failure and the need to replace the restoration. Composite materials have mechanical properties closer to natural teeth and have become a research hotspot for oral restorations. Among them, resin-infiltrated ceramic composite materials show better mechanical properties and aesthetics.
[0003] However, during the wearing process of resin-infiltrated ceramic composite materials, they may also be infected by pathogenic bacteria and cause oral diseases due to changes in the oral environment, and the material may break due to eating habits and chewing conditions. Therefore, improving the fracture resistance of resin-infiltrated ceramic composite materials, i.e. the fracture load, while giving the materials antibacterial ability, can reduce the occurrence of material fracture during service, reduce bacterial proliferation and the occurrence of oral diseases, and extend the service life of the materials.
[0004] Patent CN 108578250B discloses a method for preparing a resin-infiltrated silicate composite material. The patent prepares a ceramic block with a porous structure by controlling the sintering process, and then infiltrates the resin into the porous ceramic block by capillary action under vacuum conditions, and then solidifies to form a silicate / resin double network structure, thereby obtaining a composite material with high elastic modulus and hardness and excellent comprehensive performance. Although the composite material can improve the comprehensive performance of the restoration, it lacks antibacterial ability and still faces the problem of bacterial infection and secondary caries during use.
[0005] Patent application CN202410381819.0 discloses an antibacterial resin mixture, and uses the antibacterial resin mixture to prepare a resin-infiltrated ceramic composite material. The patent uses isothiazolinone, coupled modified nano-metal oxide and triclosan as antibacterial components. The synergistic effect of the three makes the resin-infiltrated ceramic composite material show excellent antibacterial effect on oral pathogens, but the mechanical properties of the composite material itself are basically not improved. Moreover, the applicant found in actual use that the fracture load of the antibacterial resin-infiltrated ceramic composite material is low and prone to fracture, which is also one of the main factors for clinical repair failure. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide an antibacterial resin mixture and its preparation method and application, a resin-infiltrated ceramic composite material and its preparation method. The resin-infiltrated ceramic material prepared by the antibacterial resin mixture provided by the present invention has both aesthetics and excellent antibacterial properties, and its fracture resistance is greatly improved, which can reduce the occurrence of restoration fracture and secondary caries, and extend the service life of the restoration.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides an antibacterial resin mixture, which is composed of 1-8% of an antibacterial agent, 0.1-3% of an initiator and the remainder of an acrylate monomer, in terms of mass percentage.
[0009] Taking the mass of the antibacterial agent as 100%, the antibacterial agent consists of 15-25% of isothiazolinone compounds and the remainder of polar organic solvents.
[0010] Preferably, the isothiazolinone compound is one or more of 1,2-benzisothiazolin-3-one, 2-octyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one.
[0011] Preferably, the acrylic ester monomer includes a main monomer and a diluent monomer; the mass ratio of the main monomer to the diluent monomer is (1.5-10):1.
[0012] 23. The antibacterial resin mixture according to claim 3, characterized in that the main monomer is one or more of bisphenol A-glycidyl methacrylate, ethoxylated bisphenol A dimethacrylate, N,N-dimethylaniline and carbamate dimethacrylate;
[0013] The diluent monomer is one or more of triethylene glycol dimethacrylate, ethylene glycol dimethacrylate and trimethylolpropane triacrylate.
[0014] Preferably, the initiator comprises a thermal initiator and / or a photoinitiator.
[0015] Preferably, the polar organic solvent is an ester solvent.
[0016] The present invention provides a method for preparing the antibacterial resin mixture of the above scheme, comprising the following steps: mixing an acrylic ester monomer, an initiator and an antibacterial agent to obtain the antibacterial resin mixture.
[0017] The present invention provides the use of the antibacterial resin mixture described in the above scheme or the antibacterial resin mixture prepared by the preparation method described in the above scheme in the preparation of dental materials.
[0018] Preferably, the dental material comprises an antimicrobial resin or a resin-infiltrated ceramic composite material.
[0019] The present invention provides a resin-infiltrated ceramic composite material, comprising a porous ceramic skeleton and an antibacterial resin infiltrated in the porous ceramic skeleton; the antibacterial resin is formed by curing the antibacterial resin mixture.
[0020] Preferably, the material of the porous ceramic skeleton includes any one of aluminum silicate, feldspar, silicon dioxide, zirconium oxide, tungsten oxide, nepheline and magnesium silicate, or a combination of at least two thereof.
[0021] Preferably, the porous ceramic skeleton comprises a coupled modified porous ceramic skeleton.
[0022] The present invention provides a method for preparing the resin-infiltrated ceramic composite material described in the above scheme, comprising the following steps: impregnating a porous ceramic skeleton into the above antibacterial resin mixture, performing vacuum infiltration to allow the antibacterial resin mixture to infiltrate the porous ceramic skeleton, and curing to obtain the resin-infiltrated ceramic material.
[0023] Preferably, the step of immersing the porous ceramic skeleton into the antibacterial resin mixture for vacuum infiltration includes: performing a first vacuum infiltration by immersing the antibacterial resin mixture to 1 / 3 of the height of the porous ceramic skeleton, performing a second vacuum infiltration by replenishing the antibacterial resin mixture to 2 / 3 of the porous ceramic skeleton, and performing a third vacuum infiltration by continuing to replenish the antibacterial resin mixture to completely immerse the porous ceramic skeleton.
[0024] Preferably, the pressure of the first vacuum penetration is 100-1000 Pa, and the time is 24-96 h; the pressure of the second vacuum penetration is 100-1000 Pa, and the time is 24-96 h; the pressure of the third vacuum penetration is 0.1-100 Pa, and the time is 24-96 h.
[0025] The present invention provides an antibacterial resin mixture, which is composed of 1-8% of an antibacterial agent, 0.1-3% of an initiator and the remainder of an acrylate monomer in terms of mass percentage; taking the mass of the antibacterial agent as 100%, the antibacterial agent is composed of 15-25% of an isothiazolinone compound and the remainder of a polar organic solvent. The present invention uses isothiazolinone compounds as antibacterial active ingredients, which can destroy bacterial structures, hinder bacteria from obtaining nutrients, effectively kill bacteria, reduce plaque accumulation, enhance the antibacterial ability of materials, and effectively kill Streptococcus mutans and Porphyromonas gingivalis, the main pathogens that cause caries and periodontitis; in addition, the antibacterial agent of the present invention has excellent compatibility with acrylate monomers, and the antibacterial agent has low viscosity and excellent fluidity, which can not only enhance the resin penetration ability but also promote the polymerization reaction of the resin system, thereby enhancing the mechanical properties of the material, including breaking load, strength, hardness and elastic modulus; and the refractive index of the antibacterial agent of the present invention is not significantly different from that of the ceramic skeleton, and the composite material obtained has no color difference, which enhances the aesthetic properties of the resin-infiltrated ceramic composite material. The present invention can prevent the occurrence of secondary caries while ensuring that the resin-infiltrated ceramic composite material effectively exerts the excellent performance of the material during service, thereby extending the service life of the restoration.
[0026] Another patent application of the applicant, CN202410381819.0, uses coupled modified nano-metal oxides, isothiazolinone compounds and triclosan as effective antibacterial ingredients. During actual use, it was found that the coupled modified nano-metal oxides would reduce the fracture load, elastic modulus and hardness of the resin-infiltrated ceramic composite material. Although triclosan can exert a bactericidal effect, it will reduce the degree of resin polymerization and reduce the various mechanical properties of the material, especially the fracture load. Compared with previous patent applications, the present invention omits the coupled modified nano-metal oxides and triclosan. The prepared resin-infiltrated ceramic composite material has significantly improved mechanical properties, especially the fracture load, while ensuring antibacterial and aesthetic properties, which can reduce the fracture of the restoration and extend the service life of the restoration. DETAILED DESCRIPTION
[0027] The present invention provides an antibacterial resin mixture, which is composed of 1-8% of an antibacterial agent, 0.1-3% of an initiator and the remainder of an acrylate monomer, in terms of mass percentage.
[0028] Taking the mass of the antibacterial agent as 100%, the antibacterial agent consists of 15-25% of isothiazolinone compounds and the remainder of polar organic solvents.
[0029] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0030] In terms of mass percentage, the antibacterial resin mixture provided by the present invention includes 1-8% of antibacterial agent, preferably 2-6%, more preferably 3-5%. In the embodiments of the present invention, specifically 2%, 5% or 8%.
[0031] In the present invention, the antibacterial agent is composed of an isothiazolinone compound and a polar organic solvent; the mass content of the isothiazolinone compound in the antibacterial agent is 15-25%, preferably 17-23%, and the remainder is the polar organic solvent. In an embodiment of the present invention, the mass content of the isothiazolinone compound in the antibacterial agent is specifically 15%, 20% or 25%.
[0032] In the present invention, the isothiazolinone compound is preferably one or more of 1,2-benzisothiazolin-3-one (BIT), 2-octyl-4-isothiazolin-3-one (OIT), 2-methyl-4-isothiazolin-3-one (MIT) and 5-chloro-2-methyl-4-isothiazolin-3-one (CMI), more preferably 2-octyl-4-isothiazolin-3-one (OIT); the polar organic solvent is preferably an ester solvent; the ester solvent is preferably acetate; the acetate is preferably one or more of methyl acetate, ethyl acetate, butyl acetate, glyceryl monoacetate, glyceryl diacetate and glyceryl triacetate.
[0033] The present invention uses isothiazolinone compounds as effective antibacterial ingredients, has good antibacterial effects, and has excellent compatibility with acrylate monomers, and can also promote the polymerization reaction of acrylate monomers, thereby enhancing the mechanical properties of the resin-infiltrated ceramic composite material, including breaking load, strength, hardness and elastic modulus, especially the breaking load is significantly improved.
[0034] In terms of mass percentage, the antibacterial resin mixture provided by the present invention includes 0.1-3% of initiator, preferably 0.5-2%, and more preferably 1.0-1.5%. In the present invention, the initiator includes a thermal initiator and / or a photoinitiator; the thermal initiator preferably includes one or more of benzoyl peroxide (BPO), tert-butyl peracetate, diisopropylbenzene peroxide (DCP), tert-butyl peroxy-2-ethylhexanoate (TBPO) and tert-butyl peroxybenzoate (CP-01), more preferably benzoyl peroxide (BPO); the photoinitiator preferably includes one or more of camphorquinone (CQ), di(2,4,6-trimethylbenzoyl)phenylphosphine oxide (TPO) and ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L).
[0035] The antibacterial resin mixture provided by the present invention includes a balance of acrylate monomers. In the present invention, the acrylate monomers include a main monomer and a diluent monomer; the mass ratio of the main monomer to the diluent monomer is preferably (1.5-10):1, more preferably 1.5-2.5:1. In an embodiment of the present invention, the mass ratio of the main monomer to the diluent monomer is 1.5:1 or 2.3:1. The main monomer preferably includes one or more of bisphenol A-glycidyl methacrylate (Bis-GMA), ethoxylated bisphenol A dimethacrylate (Bis-MEPP), N,N-dimethylaniline (DMA) and urethane dimethacrylate (UDMA); the diluent monomer preferably includes one or more of triethylene glycol dimethacrylate (TEGDMA), ethylene glycol dimethacrylate (EGDMA) and trimethylolpropane triacrylate (TMPTMA).
[0036] Compared with the applicant's previous patent application CN202410381819.0, the present invention omits the coupling modified nano metal oxide and triclosan. The coupling modified nano metal oxide will reduce the fracture load, elastic modulus and hardness of the resin-infiltrated ceramic composite material, and will also reduce the linear transmittance of the composite material, affecting the aesthetic performance. Although triclosan can play a bactericidal role, it will reduce the degree of resin polymerization and reduce the various mechanical properties of the material, especially the fracture load. The present invention omits the coupling modified nano metal oxide and triclosan. The mechanical properties, especially the fracture load, of the prepared resin-infiltrated ceramic composite material are significantly improved while ensuring the antibacterial and aesthetic properties, which can reduce the fracture of the restoration and extend the service life of the restoration.
[0037] The present invention provides a method for preparing the antibacterial resin mixture of the above scheme, comprising the following steps: mixing an acrylic ester monomer, an initiator and an antibacterial agent to obtain the antibacterial resin mixture.
[0038] In the present invention, the mixing preferably includes: firstly stirring the acrylic ester monomer and the initiator in a water bath at 40-60° C., then adding the antibacterial agent, and performing a second stirring.
[0039] The present invention has no special requirements for the first stirring and the second stirring, as long as the materials can be mixed evenly. In an embodiment of the present invention, the first stirring rate is 300r / min and the time is 60min; the second stirring rate is 300r / min and the time is 30min.
[0040] The present invention has no special requirements for the preparation process of the antibacterial agent, and the isothiazolinone compound and the polar organic solvent can be directly mixed thoroughly. Since the isothiazolinone compound itself has a certain viscosity, directly adding it to the resin monomer will cause the viscosity of the resin mixture to increase, which is not conducive to the penetration process, and the performance of the formed sample will decrease; the antibacterial agent formed by mixing it with the polar organic solvent in the present invention has a lower viscosity, which is conducive to the penetration of the resin mixture, thereby improving the performance.
[0041] In the present invention, after the mixing, the obtained mixture is preferably subjected to vacuum degassing. The present invention has no special requirements for the implementation process of the vacuum degassing, and the vacuum degassing process well known in the art can be used.
[0042] The present invention provides the antibacterial resin mixture described in the above scheme or the use of the antibacterial resin mixture described in the above scheme in preparing dental materials.
[0043] In the present invention, the dental material preferably comprises an antimicrobial resin or a resin-infiltrated ceramic composite material.
[0044] The dental material prepared by using the antibacterial resin mixture of the present invention has excellent antibacterial ability and aesthetic performance, as well as excellent mechanical properties, especially good fracture resistance.
[0045] The present invention provides a resin-infiltrated ceramic composite material, comprising a porous ceramic skeleton and an antibacterial resin infiltrated in the porous ceramic skeleton; the antibacterial resin is formed by curing the antibacterial resin mixture.
[0046] In the present invention, the material of the porous ceramic skeleton preferably includes any one or a combination of at least two of aluminum silicate, feldspar, silicon dioxide, zirconium oxide, tungsten oxide, nepheline and magnesium silicate; the aluminosilicate preferably includes sodium aluminum silicate.
[0047] In the present invention, the porous ceramic skeleton is preferably a coupling-modified porous ceramic skeleton, more preferably a porous ceramic skeleton modified by a silane coupling agent; the silane coupling agent preferably includes γ-methacryloxypropyltrimethoxysilane (KH570). The purpose of using the coupling-modified porous ceramic skeleton in the present invention is to increase the lipophilicity of the ceramic skeleton and promote better bonding of the antibacterial resin to the porous ceramic skeleton.
[0048] The present invention provides a method for preparing the resin-infiltrated ceramic composite material described in the above scheme, comprising the following steps: impregnating a porous ceramic skeleton into the above antibacterial resin mixture, performing vacuum infiltration to allow the antibacterial resin mixture to infiltrate the porous ceramic skeleton, and curing to obtain the resin-infiltrated ceramic material.
[0049] The present invention preferably provides a porous ceramic skeleton first. The present invention has no special requirements on the source of the porous ceramic skeleton, which can be prepared by a method well known in the art or a commercially available product.
[0050] Before the impregnation, the present invention preferably performs coupling modification on the porous ceramic skeleton; the coupling modification preferably includes the following steps: mixing the porous ceramic skeleton with a modification liquid, and then sequentially performing vacuuming, pressure holding and heat treatment; the modification liquid includes an alcohol-water mixed solvent, an acid and a coupling agent.
[0051] In the present invention, the alcohol in the alcohol-water mixed solvent preferably includes ethanol, more preferably anhydrous ethanol; the mass ratio of alcohol to water in the alcohol-water mixed solvent is preferably 1:1. The acid preferably includes any one of acetic acid, oxalic acid, hydrochloric acid, citric acid, phosphoric acid or a combination of at least two thereof; the mass of the acid is preferably 0.5-3‰ of the mass of the alcohol-water mixed solvent, more preferably 1-2.5‰; the coupling agent preferably includes a silane coupling agent, the types of which have been discussed above and will not be repeated here; the mass of the coupling agent is preferably 1-10% of the mass of the alcohol-water mixed solvent, more preferably 2-6%.
[0052] In the present invention, the mass ratio of the porous ceramic skeleton to the modifying liquid is preferably 1:3.
[0053] In the present invention, the vacuuming time is preferably 10 to 30 minutes; the pressure holding time is preferably 20 to 60 minutes. The present invention promotes the entry of the modified liquid into the pores of the porous ceramic skeleton by vacuuming and pressure holding.
[0054] In the present invention, the temperature of the heat treatment is preferably 70-90° C., more preferably 80° C., and the holding time is preferably 3-4 hours. The present invention utilizes heat treatment to promote the grafting of the coupling agent to the porous ceramic skeleton.
[0055] After the heat treatment is completed, the present invention preferably pours out the excess modification liquid, dries the modified porous ceramic skeleton, and then proceeds to the subsequent steps. In the present invention, the drying is preferably first dried at 50° C. for 1 to 3 hours, and then dried at 80° C. for 2 to 4 hours. The present invention utilizes drying to dry the modified porous ceramic skeleton.
[0056] In an embodiment of the present invention, the porous ceramic skeleton is a coupled modified porous ceramic skeleton, and the preparation method is as follows: pour 50g of sodium aluminum silicate powder into a ball mill, add 100g of ethanol and 8g of a 3% by mass polyvinyl alcohol aqueous solution for ball milling, the ball milling speed is 600r / min, the ball milling time is 2h, and then the obtained ball milled slurry is dried in a 60°C oven for 10h; sieve the powder through a 120-mesh stainless steel sieve, place the sieved powder in a molding machine, and maintain the pressure at 3MPa for 4min to obtain a ceramic green body; the ceramic green body is subjected to a secondary cold isostatic press at 220Mpa Press and hold the pressure for 2 minutes; take the ceramic body after the second pressing and place it in a sintering furnace, heat it to 800°C at a rate of 5°C / min, keep it warm for 120 minutes, and cool it to room temperature with the furnace to obtain a porous ceramic skeleton; place the porous ceramic skeleton and the modifying liquid in a beaker at a mass ratio of 1:3, evacuate the vacuum box for 20 minutes, hold the pressure for 20 minutes, place it in an oven at 80°C for 3 hours, pour out the modifying liquid, wipe off the excess modifying liquid on the surface of the ceramic skeleton, place the porous ceramic skeleton in an oven, first dry it at 50°C for 1 hour, and then dry it at 80°C for 2 hours to obtain a modified porous ceramic skeleton.
[0057] In the present invention, the step of immersing the porous ceramic skeleton into the antibacterial resin mixture for vacuum infiltration preferably includes: performing a first vacuum infiltration by immersing the porous ceramic skeleton with the antibacterial resin mixture to 1 / 3 of the height, performing a second vacuum infiltration by replenishing the antibacterial resin mixture to 2 / 3 of the porous ceramic skeleton, and performing a third vacuum infiltration by continuing to replenish the antibacterial resin mixture to completely immerse the porous ceramic skeleton.
[0058] In the present invention, the pressure of the first vacuum penetration is preferably 100 to 1000 Pa, more preferably 100 to 500 Pa, and further preferably 100 to 200 Pa; the time of the first vacuum penetration is preferably 24 to 96 hours, more preferably 48 to 96 hours, and further preferably 72 to 96 hours;
[0059] The pressure of the second vacuum penetration is preferably 100 to 1000 Pa, more preferably 100 to 500 Pa, and further preferably 100 to 200 Pa; the time of the second vacuum penetration is preferably 24 to 96 hours, more preferably 48 to 96 hours, and further preferably 72 to 96 hours;
[0060] The pressure of the third vacuum penetration is preferably 0.1 to 100 Pa, more preferably 0.1 to 1 Pa; the time of the third vacuum penetration is preferably 24 to 96 h, more preferably 48 to 96 h, further preferably 72 to 96 h.
[0061] The invention is beneficial to promoting the antibacterial resin mixture to better penetrate into the porous ceramic skeleton through step-by-step penetration.
[0062] The present invention has no special requirements for the curing conditions, and the curing conditions known in the art can be selected according to the type of initiator in the antibacterial resin mixture. In the present invention, when the initiator is a photoinitiator, the curing conditions are preferably ultraviolet light irradiation for 1 to 5 minutes; when the initiator is BPO in a thermal initiator, the curing strip preferably includes: keeping warm at 70°C for 6 hours, heating to 100°C at a rate of 2 to 5°C / min and keeping warm for 6 hours.
[0063] The antibacterial resin mixture and its preparation method and application, the resin-infiltrated ceramic composite material and its preparation method provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0064] Example 1
[0065] This embodiment provides a resin-infiltrated ceramic composite material, wherein the resin-infiltrated ceramic composite material comprises a porous ceramic skeleton and an antibacterial resin infiltrated in the porous ceramic skeleton. The preparation method of the resin-infiltrated ceramic composite material is as follows:
[0066] Preparation of antibacterial resin mixture:
[0067] (1) Weigh Bis-GMA according to Table 1 and place it in a beaker, then add TEGDMA and BPO to the beaker, and stir the solution at 300 r / min for 60 min in a 45°C water bath to make the solution uniform;
[0068] (2) Add the antimicrobial agent to the beaker and stir at 300 r / min for 30 min;
[0069] (3) The mixed resin is placed in a vacuum environment to remove bubbles therein, thereby obtaining an antibacterial resin mixture.
[0070] Preparation of porous ceramic skeleton:
[0071] (1) Pour 50 g of sodium aluminum silicate powder into a ball mill, add 100 g of ethanol and 8 g of a 3% polyvinyl alcohol aqueous solution for ball milling at a ball milling speed of 600 r / min for 2 h, and then dry the resulting ball milled slurry in an oven at 60° C. for 10 h;
[0072] (2) sieving the powder through a 120-mesh stainless steel screen, placing the sieved powder in a molding machine, and maintaining the pressure at 3 MPa for 4 minutes to obtain a ceramic green body; performing a secondary pressing on the ceramic green body in a cold isostatic press at 220 MPa, and maintaining the pressure for 2 minutes;
[0073] (3) taking the ceramic body after secondary pressing and placing it in a sintering furnace, heating it to 800° C. at a rate of 5° C. / min, keeping it at that temperature for 120 min, and cooling it to room temperature along with the furnace to obtain a porous ceramic skeleton;
[0074] (4) The porous ceramic skeleton and the modifying liquid are placed in a beaker at a mass ratio of 1:3, and the vacuum is drawn in a vacuum box for 20 minutes, and then the pressure is maintained for 20 minutes, and the ceramic skeleton is placed in an oven at 80°C for 3 hours. The modifying liquid is poured out, and the excess modifying liquid on the surface of the ceramic skeleton is wiped dry. The porous ceramic skeleton is placed in an oven, first dried at 50°C for 1 hour, and then dried at 80°C for 2 hours, and the skeleton is dried to obtain a modified porous ceramic skeleton, wherein the composition of the modifying liquid is as follows: the mass ratio of alcohol to water is 1:1, the mass of acetic acid is 1‰ of the mass of the alcohol-water mixed solvent, and the mass of KH570 is 5% of the mass of the alcohol-water mixed solvent.
[0075] Preparation of resin infiltrated ceramic composites:
[0076] (1) The antibacterial resin mixture is used to immerse 1 / 3 of the height of the modified porous ceramic skeleton, and it is placed under low vacuum infiltration at 100Pa for 72 hours. The antibacterial resin mixture is supplemented to immerse to 2 / 3 of the modified porous ceramic skeleton, and it is placed under low vacuum infiltration at 100Pa for 72 hours. The antibacterial resin mixture is supplemented to completely immerse the modified porous ceramic skeleton, and it is placed under high vacuum infiltration at 1Pa for 72 hours to obtain resin-infiltrated ceramics with good infiltration.
[0077] (2) The infiltrated resin-infiltrated ceramic is placed in an autoclave and kept at 70°C for 6 hours, and then heated to 100°C at a rate of 2°C / min and kept at this temperature for 6 hours for curing to obtain a resin-infiltrated ceramic composite material.
[0078] Embodiments 2 to 8
[0079] In each example, the resin-infiltrated ceramic composite material was prepared according to the composition ratios of the components shown in Table 1 and Table 2, and the preparation method was the same as that of Example 1.
[0080] Table 1 Antibacterial resin mixture formula in Examples 1 to 8
[0081]
[0082] Table 2 Composition of antibacterial agents of Examples 1 to 8
[0083]
[0084] Comparative Examples 1 to 7
[0085] Each comparative example provides an antibacterial resin-infiltrated ceramic composite material. The antibacterial resin of each comparative example is prepared in the same manner as in Example 1 according to the composition ratios shown in Table 3 and Table 4.
[0086] Table 3 Comparative Examples 1 to 7 Antibacterial Resin Mixture Formula
[0087]
[0088] Table 4 Composition of the composite antibacterial agent of Comparative Examples 5 to 7
[0089]
[0090] Among them, the composition of the antibacterial agent in Comparative Example 3 is the same as that in Example 3. The modified zinc oxide in Table 4 is coupled modified nano zinc oxide, and the modification method is the same as that in patent application CN202410381819.0.
[0091] Performance Testing
[0092] The antibacterial rate of the resin-infiltrated ceramic composite material prepared by the present invention against Streptococcus mutans and Porphyromonas gingivalis was tested with reference to the standard "JC / T 897-2014 Antibacterial Performance of Antibacterial Ceramic Products"; the fracture load of the resin-infiltrated ceramic composite material was tested with a Shimadzu universal tensile testing machine; the flexural strength and elastic modulus of the resin-infiltrated ceramic composite material were tested with a Shimadzu universal tensile testing machine with reference to the standard "GB 30367-2013 Dental Ceramic Materials"; the hardness of the resin-infiltrated ceramic composite material was tested with a Vickers hardness tester; the light transmittance of the resin-infiltrated ceramic composite material was tested with a haze meter with reference to the standard "YY 0271.2-2009 Dental Water-Based Cement" to verify the aesthetic properties of the material. The test results are summarized in Tables 5 and 6.
[0093] Table 5 Performance data of resin infiltrated ceramic examples
[0094]
[0095] Table 6 Performance data of comparative examples of resin infiltrated ceramics
[0096]
[0097] Analysis of the results of Examples 1 to 4 and Comparative Examples 1 to 2 shows that, compared with the case where no antibacterial agent is added, the antibacterial rates of the resin-infiltrated ceramic composite materials prepared by the present invention against oral pathogenic bacteria mutans Streptococcus and Porphyromonas gingivalis are both above 95%, and when the amount of antibacterial agent added increases, the antibacterial rate of the antibacterial resin-infiltrated ceramic is above 99%, both of which have excellent antibacterial properties. The addition of the antibacterial agent significantly enhances the mechanical properties of the resin-infiltrated ceramic, including the breaking load, elastic modulus, hardness and strength, especially the breaking load. However, when the proportion of the antibacterial agent added is too high, the mechanical properties of the resin-infiltrated ceramic will be reduced (see Comparative Example 3).
[0098] From the analysis of Example 4 and Comparative Example 5, it can be seen that the resin-infiltrated ceramics prepared by OIT-compounded triacetin alone have higher mechanical properties, including breaking load, elastic modulus and hardness, than those prepared by OIT, modified zinc oxide and triclosan-compounded triacetin. In particular, the breaking load is greatly improved, and the linear transmittance is improved, and the aesthetics is enhanced. This is mainly because zinc oxide hinders the transmission of light, and the phenolic structure of triclosan reduces the degree of polymerization of the resin. Under the joint action of the two, the promoting effect of OIT is greatly weakened, and finally the mechanical properties and aesthetic properties of the material are reduced.
[0099] Analysis of Example 2 and Comparative Example 4 shows that the use of the antibacterial ingredient OIT alone without adding a polar organic solvent will significantly reduce the aesthetic properties and mechanical properties (including breaking load, bending strength, elastic modulus and hardness) of the resin-infiltrated ceramic composite material; Analysis of Example 2 and Comparative Examples 6-7 shows that the addition of the metal oxide zinc oxide will significantly reduce the hardness, elastic modulus, breaking load and linear transmittance of the material, affecting the aesthetic properties of the material, and the addition of triclosan will significantly reduce the strength, hardness, elastic modulus and breaking load of the material; Analysis of Example 2 and Examples 7-8 shows that OIT is more compatible with the resin system of the present invention than other isothiazolinones such as MIT and CMI, and exhibits better antibacterial and mechanical properties.
[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An antibacterial resin mixture, characterized in that: Calculated by mass percentage, it is composed of 1-8% of antibacterial agent, 0.1-3% of initiator and the balance of acrylate monomer; Taking the mass of the antibacterial agent as 100%, the antibacterial agent consists of 15-25% of isothiazolinone compounds and the remainder of polar organic solvents.
2. The antibacterial resin mixture according to claim 1, characterized in that: The isothiazolinone compound is one or more of 1,2-benzisothiazolin-3-one, 2-octyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one.
3. The antibacterial resin mixture according to claim 1, characterized in that: The acrylic ester monomers include a main monomer and a diluent monomer; the mass ratio of the main monomer to the diluent monomer is (1.5-10):
1.
4. The antibacterial resin mixture according to claim 3, characterized in that: The main monomer is one or more of bisphenol A-glycidyl methacrylate, ethoxylated bisphenol A dimethacrylate, N,N-dimethylaniline and carbamate dimethacrylate; The diluent monomer is one or more of triethylene glycol dimethacrylate, ethylene glycol dimethacrylate and trimethylolpropane triacrylate.
5. The antibacterial resin mixture according to claim 1, characterized in that: The initiator includes a thermal initiator and / or a photoinitiator.
6. The antibacterial resin mixture according to claim 1, characterized in that: The polar organic solvent is an ester solvent.
7. The method for preparing the antibacterial resin mixture according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: mixing acrylic ester monomers, an initiator and an antibacterial agent to obtain the antibacterial resin mixture.
8. Use of the antibacterial resin mixture according to any one of claims 1 to 6 or the antibacterial resin mixture prepared by the preparation method according to claim 7 in the preparation of dental materials.
9. The use according to claim 8, characterized in that: The dental material includes an antimicrobial resin or a resin-infiltrated ceramic composite material.
10. A resin-infiltrated ceramic composite material, characterized in that: It comprises a porous ceramic skeleton and an antibacterial resin infiltrated in the porous ceramic skeleton; the antibacterial resin is formed by curing the antibacterial resin mixture according to any one of claims 1 to 6 or the antibacterial resin mixture prepared by the preparation method according to claim 7.
11. The resin-infiltrated ceramic composite material according to claim 10, characterized in that: The material of the porous ceramic skeleton includes any one of aluminum silicate, feldspar, silicon dioxide, zirconium oxide, tungsten oxide, nepheline and magnesium silicate, or a combination of at least two of them.
12. The resin-infiltrated ceramic composite material according to claim 10 or 11, characterized in that: The porous ceramic framework includes a coupled modified porous ceramic framework.
13. The method for preparing the resin-infiltrated ceramic composite material according to any one of claims 10 to 12, characterized in that: The following steps are involved: Dipping the porous ceramic skeleton into the antibacterial resin mixture for vacuum infiltration, so that the antibacterial resin mixture infiltrates into the porous ceramic skeleton, and solidifies to obtain the resin-infiltrated ceramic material; The antibacterial resin mixture is the antibacterial resin mixture according to any one of claims 1 to 6 or the antibacterial resin mixture prepared by the preparation method according to claim 7.
14. The preparation method according to claim 13, characterized in that: The method of immersing the porous ceramic skeleton into the antibacterial resin mixture for vacuum infiltration includes: using the antibacterial resin mixture to immerse 1 / 3 of the porous ceramic skeleton in the first vacuum infiltration, replenishing the antibacterial resin mixture to 2 / 3 of the porous ceramic skeleton for the second vacuum infiltration, and continuing to replenish the antibacterial resin mixture to completely immerse the porous ceramic skeleton for the third vacuum infiltration.
15. The preparation method according to claim 14, characterized in that: The pressure of the first vacuum penetration is 100-1000 Pa, and the time is 24-96 hours; the pressure of the second vacuum penetration is 100-1000 Pa, and the time is 24-96 hours; the pressure of the third vacuum penetration is 0.1-100 Pa, and the time is 24-96 hours.
Citation Information
Patent Citations
A resin-infiltrated silicate composite material and its preparation and application
CN108578250B
Antibacterial resin mixture and preparation method and application thereof, antibacterial resin, elastic ceramic material and preparation thereof, resin permeable ceramic material and preparation thereof, and dental prosthesis
CN118255931A
Cited By
Antibacterial resin mixture, and preparation method therefor and use thereof
EP4768510A1
Antibacterial resin mixture, and preparation method therefor and use thereof
WO2025200694A1