Spherical silicon-carbon negative electrode material and preparation method thereof

Through the combined structure of porous spherical doped hard carbon substrate, nanosilicon deposition and carbon cladding of spherical silicon carbon anode material, combined with element doping, the volume expansion and circulation performance in silicon carbon technology in lithium-ion batteries is solved. The problem has achieved the improvement of high specific capacity and cycle stability, and simplified industrial production.

CN118983416APending Publication Date: 2024-11-19合肥国轩新材料科技有限公司
View PDF 0 Cites 16 Cited by

Patent Information

Application Number
CN202411070857.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In current lithium-ion batteries, the fourth-generation vapor-phase deposition silicon carbon technology faces difficulties in the preparation of porous carbon carbon skeletons, silane deposition and carbon coating processes, resulting in problems such as material volume expansion and poor circulation performance, and has high technical thresholds and industries. Defective difficulties.

Method used

The spherical silicon carbon negative electrode material is used to improve the bonding of silicon and carbon base and the conductivity of the material through a combined structure of porous spherical doping hard carbon substrate, nano-silicon deposition and carbon cladding layer. Reduce volume expansion and improve cycle stability.

Benefits of technology

It has achieved the improvement of high specific capacity, cycle stability and service life, and at the same time, it has simplified industrial production, solved the problems of volume expansion and poor circulation performance of silicon carbon negative electrode materials, reduced internal resistance and improved the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983416A_ABST
    Figure CN118983416A_ABST
Patent Text Reader

Abstract

The invention provides a spherical silicon-carbon negative electrode material and a preparation method thereof. The spherical silicon-carbon negative electrode material comprises a porous spherical doped hard carbon substrate, nano silicon dispersed and filled in pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate. According to the spherical silicon-carbon negative electrode material and the preparation method thereof provided by the invention, the problems of porous hard carbon precursor synthesis, silane deposition, carbon coating process and the like in the current vapor deposition silicon-carbon technology are solved, and the problems of volume expansion, poor cycle performance and the like of the existing silicon are solved from the aspects of element doping and structural design.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a spherical silicon-carbon negative electrode material and a preparation method thereof. Background Art

[0002] With the rapid development of consumer electronics, electric vehicles and electrochemical energy storage industries, people are increasingly demanding high-energy-density lithium-ion batteries. Traditional graphite anode materials are no longer able to meet the current situation due to their limited theoretical specific capacity (372mAh / g). Developing high-energy-density anode materials to replace traditional graphite-based carbon-based materials is one of the important research directions for improving the energy density of lithium-ion batteries.

[0003] Elemental silicon has attracted widespread attention due to its abundant earth reserves, the highest known theoretical specific capacity (4200mAh / g), and high lithium insertion potential. However, silicon negative electrode materials themselves also have problems such as volume expansion after lithium insertion, material crushing, performance degradation after multiple cycles, and capacity loss due to SEI formation. From a commercial perspective, the silicon negative electrode material industry continues to tackle key problems, and the main technical development paths are sand-milled silicon carbon (first generation), conventional coated silicon oxygen (second generation), pre-lithium and pre-magnesium silicon oxygen (third generation), and vapor deposited silicon carbon (fourth generation). With the continuous iteration and breakthroughs in technology, silicon negative electrode materials have become the next generation of lithium battery negative electrode materials widely accepted by the market, providing great support for further improving the energy density of lithium batteries and further penetrating them into new energy vehicles.

[0004] At present, the fourth generation of vapor-deposited silicon-carbon technology has three main difficulties: (1) Preparation of porous carbon-carbon skeleton. As the substrate for silicon deposition, the carbon skeleton must have a porous structure to accommodate silicon, and must have a certain structural stability to accommodate the volume expansion of silicon. In addition, it must have a certain batch stability. (2) Deposition of silicon particles inside the porous carbon. The deposition of silane inside the porous carbon is generally divided into two steps: adsorption and deposition (cracking). The current mainstream in the industry uses a fluidized bed as a reactor to achieve the uniformity of silane adsorption and cracking inside the porous carbon as much as possible, and finally obtain nano-silicon particles. (3) Carbon layer coating. After the silicon particles are deposited, a carbon-source gas will be introduced into the fluidized bed to uniformly coat the surface of the material with a carbon layer to improve the electrical conductivity of the overall material and reduce side reactions, and finally obtain vapor-deposited silicon-carbon.

[0005] It can be seen that the technical barriers and industrial difficulties of vapor deposition silicon carbon technology mainly lie in the selection of porous carbon, deposition equipment and deposition process, which involves unique raw materials, equipment and processes and has extremely high technical thresholds. Summary of the invention

[0006] Based on the technical problems existing in the background technology, the present invention proposes a spherical silicon-carbon negative electrode material and a preparation method thereof, which overcomes the difficulties of porous hard carbon precursor synthesis, silane deposition and carbon coating process existing in the current vapor deposition silicon-carbon technology, and overcomes the problems of volume expansion and poor cycle performance faced by existing silicon from the level of element doping and structural design.

[0007] The present invention provides a spherical silicon-carbon negative electrode material, which comprises a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0008] In the present invention, the negative electrode material includes a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate; on the one hand, the presence of the porous spherical doped hard carbon substrate improves the bonding between silicon and the porous hard carbon substrate during silane deposition, and silicon can effectively fill excess pores, thereby reducing internal resistance while obtaining a higher specific capacity, and while ensuring the high specific capacity of the negative electrode material, it can also improve the cycle stability and service life of the battery; on the other hand, the spherical design of the negative electrode material further improves the transmission of lithium ions, inhibits the volume expansion of the negative electrode material during the lithium insertion process, and lithium precipitation caused by local overpotential.

[0009] Preferably, the doping element of the porous spherical doped hard carbon substrate is at least one of boron, titanium or phosphorus.

[0010] In the present invention, element doping not only improves the ion and electron conductivity of the negative electrode material, but also ensures a high specific capacity of the negative electrode material.

[0011] Preferably, based on the total mass of the negative electrode material, the carbon content is 45-60%, the silicon content is 35-50%, and the doping element content is 1-5%.

[0012] Preferably, the particle size of the porous spherical doped hard carbon substrate is 0.5-10 μm, the particle size of the nano-silicon is 2-40 nm, and the thickness of the carbon coating layer is 5-30 nm.

[0013] The present invention also provides a method for preparing the spherical silicon-carbon negative electrode material, comprising the following steps:

[0014] S1, emulsifying and polymerizing a phenolic resin prepolymer, a surfactant, a curing agent and an aldehyde compound to obtain phenolic resin microspheres; pre-carbonizing the phenolic resin microspheres and mixing them with a doping source, and carbonizing them to obtain a porous spherical doped hard carbon substrate;

[0015] S2, introducing silicon source gas into the porous spherical doped hard carbon substrate to perform silicon vapor deposition to obtain a silicon-carbon core;

[0016] S3, introducing a carbon source gas into the silicon-carbon core for carbon coating deposition, thereby obtaining the spherical silicon-carbon negative electrode material.

[0017] In the present invention, phenolic resin prepolymer, surfactant, curing agent and aldehyde compound are emulsified and polymerized. The phenolic resin prepolymer is cross-linked and polymerized with the aldehyde compound under the condition of curing agent under the premise of surfactant as template, which not only controls the formation of porous structure of the obtained phenolic resin, but also helps the obtained phenolic resin to obtain spherical morphology, and the size is controlled within ten microns, and finally forms a spherical silicon-carbon negative electrode material. The high sphericity of the spherical negative electrode material is beneficial to ensure the strength of the material and maintain the integrity of the negative electrode structure, thereby improving the performance and life of the battery, and is also beneficial to improving the specific surface area of ​​the silicon composite negative electrode material. area, increasing the number of active sites that can insert and deinsert lithium, which is beneficial to the improvement of the first coulombic efficiency of the silicon-carbon composite negative electrode material; thereafter, nano-silicon is generated by pyrolysis of the silicon source and deposited into the pores of the porous spherical doped hard carbon substrate to obtain a silicon-carbon core, and the overall capacity of the silicon-carbon negative electrode material is improved by utilizing the high theoretical specific capacity of silicon; finally, the carbon source gas is in situ pyrolyzed into a carbon layer and coated on the surface of the silicon-carbon core. Since the in situ formed carbon layer is tightly coated on the surface of the silicon-carbon core, it not only alleviates the volume expansion of the silicon-carbon negative electrode material during use, but also improves the conductivity of the negative electrode material, thereby effectively improving the cycle performance.

[0018] Preferably, in step S1, the surfactant is at least one of Span 80, Triton X-100, lecithin P123 or hexadecyltrimethylammonium bromide; the curing agent is at least one of ethylenediamine, triethylamine, trimethylamine, tripropylamine, diethylethanolamine or hexamethylenetetramine; the aldehyde compound is at least one of formaldehyde, malondialdehyde, succindialdehyde, glutaraldehyde, 2-hydroxyglutaraldehyde, β-methylglutaraldehyde, adipaldehyde, heptanedialdehyde, suberaldehyde or maleic aldehyde;

[0019] Preferably, the emulsion polymerization temperature is 60-100° C. and the time is 3-12 hours.

[0020] Preferably, in step S1, the doping source is at least one of boric acid, phosphoric acid or titanic acid;

[0021] Preferably, the pre-carbonization temperature is 700-900°C, and the time is 1-3h; the carbonization temperature is 700-900°C, and the time is 12-48h.

[0022] Preferably, in step S2, the silicon source gas includes silane, acetylene and an inert gas;

[0023] Preferably, the silane is at least one of monosilane, disilane, dimethylsilane or dichlorosilane, and the inert gas is at least one of nitrogen, argon or helium;

[0024] Preferably, in the silicon source gas, the volume content of silane is 20-40%, the volume content of acetylene is 5-10%, and the volume content of inert gas is 40-70%;

[0025] Preferably, the temperature of the silicon vapor deposition is 520-600° C. and the time is 2-4 hours.

[0026] Preferably, in step S3, the carbon source gas includes alkanes and inert gases;

[0027] Preferably, the alkane is at least one of methane, ethane, acetylene, ethylene or propylene, and the inert gas is at least one of nitrogen, argon or helium;

[0028] Preferably, in the carbon source gas, the volume content of alkanes is 50-70%, and the volume content of inert gas is 30-50%;

[0029] Preferably, the carbon deposition coating is carried out at a temperature of 700-850° C. and for a time of 2-5 hours.

[0030] The present invention also provides a lithium ion battery, comprising the above negative electrode material or the negative electrode material prepared by the above preparation method.

[0031] Compared with the prior art, the beneficial technical effects achieved by the present invention are as follows:

[0032] (1) The spherical silicon-carbon negative electrode material of the present invention includes a porous spherical hard carbon substrate located inside, silicon nanoparticles dispersed in the pores of the substrate, and a carbon coating layer coated on the outer layer of the substrate; the spherical structure of the negative electrode material provides a stable skeleton, and the hard carbon substrate synthesized by the resin base has the advantages of high material consistency, easy control of pore size, and high uniformity of nano-silicon deposition.

[0033] (2) The spherical silicon-carbon negative electrode material of the present invention not only improves the ionic and electronic conductivity of the material through element doping and carbon coating, but also improves the binding property of silicon and carbon base during silane deposition, effectively fills the excess pores, reduces the internal resistance and has a higher specific capacity. While ensuring the high specific capacity of the silicon-carbon negative electrode material, it improves the cycle stability and service life of the battery.

[0034] (3) The preparation method of the present invention is conducive to industrial production and effectively solves the commercial application problems in the current lithium battery industry, such as the synthesis of spherical hard carbon substrate materials, uniform deposition of silicon, carbon coating and material consistency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a SEM image of the spherical silicon-carbon negative electrode material described in Example 1 of the present invention;

[0036] Figure 2 1 and 2 are XRD diagrams of the spherical silicon-carbon negative electrode materials described in Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0037] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0038] Example 1

[0039] This embodiment provides a spherical silicon-carbon negative electrode material, including a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0040] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0041] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt%) of 30 wt % of the mass of the phenolic resin prepolymer. After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 80° C., curing reaction for 8 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0042] The phenolic resin microspheres are heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 hours, and then the pre-carbonized phenolic resin microspheres and boric acid are mixed in a mass ratio of 3:1. After drying, the mixture is heated to 800° C. in a carbon dioxide atmosphere and carbonized for 36 hours to obtain a porous spherical doped hard carbon substrate.

[0043] (2) placing the porous spherical doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of monosilane, acetylene and nitrogen in a volume ratio of 5:1:13, heating to 550°C, and causing monosilane to decompose at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 3 hours, a silicon-carbon core is obtained;

[0044] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 725°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 3 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0045] The spherical silicon-carbon negative electrode material obtained in Example 1 was scanned by electron microscope. The results are as follows: Figure 1 As shown, Figure 1 is a SEM image of the spherical silicon-carbon negative electrode material described in Example 1 of the present invention; Figure 1 It can be seen that the negative electrode material described in this embodiment is spherical.

[0046] Example 2

[0047] This embodiment provides a spherical silicon-carbon negative electrode material, including a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0048] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0049] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt%) of 30 wt % of the mass of the phenolic resin prepolymer. After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 80° C., curing reaction for 8 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0050] The phenolic resin microspheres are heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 hours, and then the pre-carbonized phenolic resin microspheres and boric acid are mixed in a mass ratio of 4:1. After drying, the mixture is heated to 800° C. in a carbon dioxide atmosphere and carbonized for 48 hours to obtain a porous spherical doped hard carbon substrate.

[0051] (2) placing the porous spherical doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing silicon source gas of disilane, acetylene and nitrogen in a volume ratio of 3:1:6, heating to 520°C, and silane is cracked at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 4 hours, a silicon-carbon core is obtained;

[0052] (3) The silicon source gas is replaced with a carbon source gas of methane and nitrogen in a volume ratio of 3:2, and the temperature is raised to 700°C. Acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 3 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0053] Example 3

[0054] This embodiment provides a spherical silicon-carbon negative electrode material, including a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0055] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0056] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), hexadecyltrimethylammonium bromide and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt %) of 30 wt % of the mass of the phenolic resin prepolymer. After the dripping is complete for 30 minutes, stirring at a rate of 500 r / min and heating to 100° C., curing reaction for 3 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0057] The phenolic resin microspheres were heated to 700° C. in a nitrogen atmosphere, pre-carbonized for 3 h, and then the pre-carbonized phenolic resin microspheres and titanic acid were mixed in a mass ratio of 3:1. After drying, the mixture was heated to 900° C. in a carbon dioxide atmosphere and carbonized for 24 h to obtain a porous spherical doped hard carbon substrate.

[0058] (2) placing the porous spherical doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of dimethylsilane, acetylene and nitrogen in a volume ratio of 2:1:7, heating to 600°C, and causing monosilane to decompose at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 2 hours, a silicon-carbon core is obtained;

[0059] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 850°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 2 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0060] Example 4

[0061] This embodiment provides a spherical silicon-carbon negative electrode material, including a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0062] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0063] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping 15wt% of succinaldehyde (15wt% of the mass of the phenolic resin prepolymer). After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 60°C, curing reaction for 12 hours, filtering, and placing the obtained polymer microspheres in a drying oven at 95°C for 12 hours to obtain phenolic resin microspheres;

[0064] The phenolic resin microspheres are heated to 900° C. in a nitrogen atmosphere, pre-carbonized for 1 hour, and then the pre-carbonized phenolic resin microspheres and boric acid are mixed in a mass ratio of 3:1. After drying, the mixture is heated to 700° C. in a carbon dioxide atmosphere and carbonized for 48 hours to obtain a porous spherical doped hard carbon substrate.

[0065] (2) placing the porous spherical doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of dichlorosilane, acetylene and nitrogen in a volume ratio of 8:1:11, heating to 550° C., and causing monosilane to decompose at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 4 hours, a silicon-carbon core is obtained;

[0066] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 725°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 5 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0067] Example 5

[0068] This embodiment provides a spherical silicon-carbon negative electrode material, including a porous spherical doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

[0069] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0070] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 30:1:1.4, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt%) of 30 wt % of the mass of the phenolic resin prepolymer. After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 80° C., curing reaction for 8 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0071] The phenolic resin microspheres are heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 hours, and then the pre-carbonized phenolic resin microspheres and boric acid are mixed in a mass ratio of 3:1. After drying, the mixture is heated to 800° C. in a carbon dioxide atmosphere and carbonized for 36 hours to obtain a porous spherical doped hard carbon substrate.

[0072] (2) placing the porous spherical doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of monosilane, acetylene and nitrogen in a volume ratio of 5:1:13, heating to 550°C, and causing monosilane to decompose at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 3 hours, a silicon-carbon core is obtained;

[0073] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 725°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 3 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0074] Comparative Example 1

[0075] This comparative example proposes a spherical silicon-carbon negative electrode material, comprising a porous spherical hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical hard carbon substrate.

[0076] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0077] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt%) of 30 wt % of the mass of the phenolic resin prepolymer. After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 80° C., curing reaction for 8 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0078] The phenolic resin microspheres were heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 h, and then heated to 800° C. in a carbon dioxide atmosphere and carbonized for 36 h to obtain a porous spherical hard carbon substrate;

[0079] (2) placing the porous spherical hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of monosilane, acetylene and nitrogen in a volume ratio of 5:1:13, heating to 550°C, and pyrolyzing monosilane at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical hard carbon substrate. After deposition for 3 hours, a silicon-carbon core is obtained;

[0080] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 725°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 3 hours, the carbon layer is naturally cooled to room temperature to obtain the spherical silicon-carbon negative electrode material.

[0081] Comparative Example 2

[0082] This comparative example proposes a spherical silicon-carbon negative electrode material, comprising a porous spherical doped hard carbon substrate and nano-silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate.

[0083] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0084] (1) adding a phenolic resin prepolymer (obtained by polymerization of phenol and formaldehyde in a molar ratio of 1:1, with an average molecular weight of 400), Span 80 and hexamethylenetetramine to tetraethyl orthosilicate (4 times the mass of the phenolic resin prepolymer) in a mass ratio of 15:1:0.7, stirring and mixing at a rate of 500 r / min for 1 hour, and then dripping a formaldehyde aqueous solution (37 wt%) of 30 wt % of the mass of the phenolic resin prepolymer. After 30 minutes of dripping, stirring at a rate of 500 r / min and heating to 80° C., curing reaction for 8 hours, suction filtering, and placing the obtained polymer microspheres in a drying oven at 95° C. for 12 hours to obtain phenolic resin microspheres;

[0085] The phenolic resin microspheres are heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 hours, and then the pre-carbonized phenolic resin microspheres and boric acid are mixed in a mass ratio of 3:1. After drying, the mixture is heated to 800° C. in a carbon dioxide atmosphere and carbonized for 36 hours to obtain a porous spherical doped hard carbon substrate.

[0086] (2) The porous spherical doped hard carbon substrate is placed in a fluidized bed reactor, and after nitrogen is introduced for 30 minutes, a silicon source gas of monosilane, acetylene and nitrogen with a volume ratio of 5:1:13 is introduced, and the temperature is raised to 550°C. Under high temperature, monosilane is cracked to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 3 hours, the spherical silicon-carbon negative electrode material is obtained.

[0087] The spherical silicon-carbon negative electrode materials obtained in Example 1 and Comparative Example 2 were subjected to X-ray diffraction. The results are as follows: Figure 2 As shown, Figure 2 The XRD diagrams of the spherical silicon-carbon negative electrode materials described in Example 1 and Comparative Example 2 of the present invention are shown in FIG. Figure 2 It can be seen that the spherical silicon-carbon negative electrode material described in Example 1 has no characteristic peaks of silicon, that is, there are no characteristic crystallization peaks near the positions of 28.4°, 47.3°, and 56.1°. At the same time, compared with Comparative Example 2, the uncoated spherical silicon-carbon negative electrode material has obvious silicon characteristic peaks.

[0088] Comparative Example 3

[0089] This comparative example proposes a silicon-carbon negative electrode material, comprising a porous doped hard carbon substrate, nano-silicon dispersedly filled in the pores of the porous doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous doped hard carbon substrate.

[0090] The preparation method of the spherical silicon-carbon negative electrode material specifically includes:

[0091] (1) Phenol, formaldehyde aqueous solution (37 wt%) and sodium hydroxide were mixed in a molar ratio of 1:1:0.01, stirred at a rate of 500 r / min for 1 hour, heated to 80° C., cured for 12 hours, filtered, and the obtained polymer powder was placed in a drying oven at 95° C. and dried for 12 hours to obtain a phenolic resin powder;

[0092] The phenolic resin powder is heated to 800° C. in a nitrogen atmosphere, pre-carbonized for 2 hours, and then the pre-carbonized phenolic resin powder and boric acid are mixed in a mass ratio of 3:1. After drying, the mixture is heated to 800° C. in a carbon dioxide atmosphere and carbonized for 36 hours to obtain a porous doped hard carbon substrate.

[0093] (2) placing the porous doped hard carbon substrate in a fluidized bed reactor, introducing nitrogen for 30 minutes, and then introducing a silicon source gas of monosilane, acetylene and nitrogen in a volume ratio of 5:1:13, heating to 550°C, and causing monosilane to decompose at high temperature to form nano-silicon particles, which are deposited in the pores of the porous spherical doped hard carbon substrate. After deposition for 3 hours, a silicon-carbon core is obtained;

[0094] (3) The silicon source gas is replaced with a carbon source gas of acetylene and nitrogen in a volume ratio of 1:1, and the temperature is raised to 725°C. The acetylene is cracked at high temperature to form a carbon layer, which is deposited and coated on the surface of the silicon-carbon core. After deposition for 3 hours, the carbon layer is naturally cooled to room temperature to obtain the silicon-carbon negative electrode material.

[0095] The silicon-carbon negative electrode material obtained in the embodiment and the comparative example was mixed with conductive carbon black (SP), single-walled carbon nanotubes (SWCNT), sodium tridecanol (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 90:1.45:0.05:2:6.5 to form a slurry, evenly coated on a copper foil, dried at 70°C for 12 h, and then punched out a button electrode sheet with a diameter of 12 mm using a punching machine; then metallic lithium was used as the negative electrode, Cellgard2400 microporous polypropylene membrane was used as the diaphragm, and 1 mol / L LiPF6 solution (the solvent was ethylene carbonate EC / dimethyl carbonate DMC, v / v=1:1) was used as the electrolyte, and a 2032-type button battery was assembled in an argon atmosphere glove box.

[0096] The button cell was placed on a LAND battery tester for electrochemical performance testing, with a charge and discharge voltage range of 0.01-1.5V and a charge and discharge current of 0.1C. The results are listed in Table 1; wherein, the first expansion rate of the electrode is the ratio of the thickness of the active material layer after the first lithium removal to the thickness of the active material layer before lithium insertion.

[0097] Table 1 Electrochemical test results of silicon-carbon negative electrode materials obtained in Examples and Comparative Examples

[0098]

[0099] Based on the above table, from the comparison results of Example 1 and Comparative Example 1, it can be seen that the first delithiation capacity of the spherical silicon-carbon material described in Example 1 is 1931.3 mAh / g, while the first delithiation capacity of Comparative Example 1 is reduced to 1891.3 mAh / g due to the lack of doped elements; and because element doping can effectively improve the bonding ability of Si and C, improve the stable and uniform deposition of silicon in the hard carbon substrate, and reduce the specific surface area and powder resistance of the material, the powder resistance of the undoped Comparative Example 1 is reduced from 78Ω·cm to 6.1Ω·cm of Example 1, showing better electronic conductivity; in addition, the structure of the negative electrode material after element doping is more stable, which is reflected in the fact that the expansion of the pole piece is reduced from 65.7% of the undoped Comparative Example 1 to 43.3% after doping, showing a more excellent low expansion coefficient.

[0100] In addition, from the comparison results of Example 1 and Comparative Example 3, it can be seen that although the negative electrode materials of both use phenolic resin as the carbon source, the spherical silicon-carbon negative electrode material described in Example 1 has a higher first coulombic efficiency, as well as lower powder resistance and first electrode expansion rate; this is because in Example 1, the spherical regularity of the obtained hard carbon substrate can be well controlled, and its size can be smaller and the compaction density can be higher, which is beneficial to increasing the specific surface area of ​​the negative electrode material and increasing the number of active sites that can be deintercalated and deintercalated lithium, thereby facilitating the improvement of the first coulombic efficiency of the silicon-carbon composite negative electrode material and the reduction of the electrode expansion rate, etc.; whereas in Comparative Example 1, since the hard carbon substrate is obtained by direct phenolic polymerization, it cannot control the formation of a spherical morphology, which is not conducive to the subsequent improvement of battery performance.

[0101] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A spherical silicon-carbon negative electrode material, characterized in that: The invention comprises a porous spherical doped hard carbon substrate, nano silicon dispersedly filled in the pores of the porous spherical doped hard carbon substrate, and a carbon coating layer coated on the surface of the porous spherical doped hard carbon substrate.

2. The spherical silicon-carbon negative electrode material according to claim 1, characterized in that: The doping element of the porous spherical doped hard carbon substrate is at least one of boron, titanium or phosphorus.

3. The spherical silicon-carbon negative electrode material according to claim 1 or 2, characterized in that: Based on the total mass of the negative electrode material, the carbon content is 45-60%, the silicon content is 35-50%, and the doping element content is 1-5%.

4. The spherical silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The particle size of the porous spherical doped hard carbon substrate is 0.5-10 μm, the particle size of the nano-silicon is 2-40 nm, and the thickness of the carbon coating layer is 5-30 nm.

5. A method for preparing the spherical silicon-carbon negative electrode material according to any one of claims 1 to 4, characterized in that: The steps include: S1, emulsifying and polymerizing a phenolic resin prepolymer, a surfactant, a curing agent and an aldehyde compound to obtain phenolic resin microspheres; pre-carbonizing the phenolic resin microspheres and mixing them with a doping source, and carbonizing them to obtain a porous spherical doped hard carbon substrate; S2, passing a silicon source gas into the porous spherical doped hard carbon substrate to perform silicon vapor deposition to obtain a silicon-carbon core; S3, introducing a carbon source gas into the silicon-carbon core for carbon coating deposition, thereby obtaining the spherical silicon-carbon negative electrode material.

6. The method for preparing the spherical silicon-carbon negative electrode material according to claim 5, characterized in that: In step S1, the surfactant is at least one of Span 80, Triton X-100, lecithin P123 or hexadecyltrimethylammonium bromide; the curing agent is at least one of ethylenediamine, triethylamine, trimethylamine, tripropylamine, diethylethanolamine or hexamethylenetetramine; the aldehyde compound is at least one of formaldehyde, malondialdehyde, succindialdehyde, glutaraldehyde, 2-hydroxyglutaraldehyde, β-methylglutaraldehyde, adipaldehyde, heptanedialdehyde, suberaldehyde or maleic aldehyde; Preferably, the emulsion polymerization temperature is 60-100° C. and the time is 3-12 hours.

7. The method for preparing the spherical silicon-carbon negative electrode material according to claim 5 or 6, characterized in that: In step S1, the doping source is at least one of boric acid, phosphoric acid or titanic acid; Preferably, the pre-carbonization temperature is 700-900°C, and the time is 1-3h; the carbonization temperature is 700-900°C, and the time is 12-48h.

8. The method for preparing the spherical silicon-carbon negative electrode material according to any one of claims 5 to 7, characterized in that: In step S2, the silicon source gas includes silane, acetylene and an inert gas; Preferably, the silane is at least one of monosilane, disilane, dimethylsilane or dichlorosilane, and the inert gas is at least one of nitrogen, argon or helium; Preferably, in the silicon source gas, the volume content of silane is 20-40%, the volume content of acetylene is 5-10%, and the volume content of inert gas is 40-70%; Preferably, the temperature of the silicon vapor deposition is 520-600° C. and the time is 2-4 hours.

9. The method for preparing the spherical silicon-carbon negative electrode material according to any one of claims 5 to 8, characterized in that: In step S3, the carbon source gas includes alkanes and inert gases; Preferably, the alkane is at least one of methane, ethane, acetylene, ethylene or propylene, and the inert gas is at least one of nitrogen, argon or helium; Preferably, in the carbon source gas, the volume content of alkanes is 50-70%, and the volume content of inert gas is 30-50%; Preferably, the carbon deposition coating is carried out at a temperature of 700-850° C. and for a time of 2-5 hours.

10. A lithium ion battery, characterized in that: The invention comprises the negative electrode material according to any one of claims 1 to 4 or the negative electrode material prepared by the preparation method according to any one of claims 5 to 9.

Citation Information

Cited By

  • Preparation method of aerogel spherical porous carbon, preparation method of aerogel spherical silicon carbon negative electrode material and battery

    CN119735206A

  • System and process method capable of continuously preparing high-gram-volume and low-expansion silicon-carbon material

    CN120054376A

  • A system and process method for continuously preparing high specific capacity and low expansion silicon-carbon materials

    CN120054376B

  • Spherical silicon-carbon negative electrode material and preparation method and application thereof

    CN120184229A

  • A spherical silicon-carbon negative electrode material and its preparation method and application

    CN120184229B