Pd-coated NiCo spinel catalyst based on directional loading of PBA carrier as well as preparation method and application of Pd-coated NiCo spinel catalyst

By orientedly loading Pd ions on the PBA support and exchanging them with NiCoPBA to form a Pd@NiCo spinel catalyst, the problem of insufficient low-temperature activity of the catalyst is solved, the high dispersion and oxygen activation ability of the catalyst are improved, and the catalysis is significantly improved performance.

CN118988342APending Publication Date: 2024-11-22NANJING UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411026802.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing PBA-derived catalysts have shortcomings in low-temperature activity, especially the dispersion and active site exposure of precious metal Pd, which leads to limited catalytic performance.

Method used

Using a directional loading method based on PBA support, the Pd ions and highly ordered Ni2+ clusters in NiCoPBA are exchanged through alkali-assisted ion exchange to form a Pd@NiCo spinel catalyst, and the oxygen bridge connection is used to enhance the interaction between metal and support, thereby enhancing the catalyst's interaction. Dispersibility and oxygen activation ability.

Benefits of technology

The low-temperature activity and oxygen activation ability of Pd@NiCo spinel catalyst were significantly improved, and the catalytic performance was improved, especially in the process of catalytic oxidation of toluene in VOCs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988342A_ABST
    Figure CN118988342A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of VOCs catalytic oxidation catalysts, in particular to a Pd-coated NiCo spinel catalyst based on directional loading of a PBA carrier and a preparation method and application of the Pd-coated NiCo spinel catalyst. According to the preparation method, the advantages of an ion exchange method and an MOFs derivation method are effectively coupled based on the structure reversible characteristic of NiCoPBA and the highly ordered characteristic of Ni < 2 + > clusters, and the Pd-coated NiCo spinel catalyst which has high-dispersion Pd active sites and is similar to NiCoPBA in morphology is prepared. The high-dispersion Pd active sites of the catalyst and the characteristic similar to NiCoPBA morphology are beneficial to promoting O2 molecules to dissociate on the Pd active sites to form active oxygen species; meanwhile, Pd is uniformly embedded into the NiCo spinel catalyst, the mobility of active oxygen species is effectively improved, and a large number of oxygen vacancies are formed in situ, so that the oxygen activation capacity of the Pd-coated NiCo spinel catalyst is remarkably improved. Therefore, the Pd-coated NiCo spinel catalyst shows excellent low-temperature activity and good stability in catalytic oxidation of VOCs, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of VOCs catalytic oxidation catalyst preparation, and in particular to a Pd@NiCo spinel catalyst based on PBA carrier directional loading, and a preparation method and application thereof. Background Art

[0002] Catalytic combustion is one of the preferred technologies for VOCs terminal treatment, in which the catalyst itself is the key to the process. Prussian blue analogue (PBA) has become an important precursor for the preparation of related catalysts due to its economy, porous structure and good designability.

[0003] For PBA-derived catalysts, the current technical difficulty is how to further reduce the low-temperature activity of the catalyst.

[0004] Introducing a small amount of precious metal into spinel catalysts is an effective method to improve their low-temperature activity. Among them, metal Pd is an excellent choice due to its unique electronic structure and relatively low price compared to Pt. Generally, improving the dispersibility of precious metal Pd is conducive to exposing more Pd active sites, thereby improving reaction efficiency, while also strengthening the metal-support interaction and improving the intrinsic activity of the catalyst. However, the above modification strategy still has the following technical difficulties:

[0005] 1) How to effectively control the surface defects of spinel to enhance the interaction between metal and support, thereby improving the intrinsic activity of catalytic active centers;

[0006] 2) For noble metal @ metal oxide catalysts, improving the dispersion of noble metals is beneficial to the full contact between reactants and noble metal active centers, thereby improving catalytic performance. However, the high surface energy of highly dispersed noble metals causes them to tend to aggregate. Therefore, highly dispersed noble metal @ metal oxide catalysts are still a problem in the synthesis process.

[0007] In order to solve the above problems, the present invention designs a Pd@NiCo spinel catalyst based on a directional loading of a PBA carrier, a preparation method and an application thereof. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a Pd@NiCo spinel catalyst based on a PBA carrier. In this scheme, PBA (with a general structural formula of A) in the MOFs family is used. x The reversible characteristics of [B(CN)6]y·m H2O) can realize the exchange of Pd ions with the A site in PBA with the assistance of alkali, so that the Pd ions occupy the A site in PBA. Based on the highly ordered characteristics of the A site itself, the Pd clusters in the Pd@NiCo spinel catalyst after ion exchange also have highly ordered characteristics, thereby realizing the directional loading of Pd on PBA. The specific scheme is as follows:

[0009] In a first aspect, the present invention provides a Pd@NiCo spinel catalyst.

[0010] The present invention designs a Pd@NiCo spinel catalyst based on a PBA carrier directional loading, and the periodic structure with complete functions includes:

[0011] Spinel, which inherits the microstructure of PBA support and has oxygen vacancies, and metal clusters connected to the spinel support through oxygen bridges;

[0012] There is a strong metal-support interaction between the metal clusters and the spinel;

[0013] The PBA carrier is a NiCoPBA carrier; the metal cluster is a Pd cluster, and its particle size ranges from 1 to 20 nm; the spinel is a NiCo spinel;

[0014] The surface area of ​​the Pd@NiCo spinel catalyst is 134.6 m 2 / g, the average pore size is 0.28cm 3 / g, and the average pore size is 17.92nm.

[0015] Description: For noble metal@metal oxide catalysts, the formation of abundant oxygen vacancies and strong metal-support interactions are beneficial to improving their low-temperature activity. The present invention utilizes base-assisted ion exchange to achieve Pd 2+ The highly ordered Ni in NiCoPBA 2+ The exchange of clusters with changes the coordination environment of the original NiCoPBA, which is conducive to the formation of abundant oxygen vacancies in the derivatization process of NiCoPBA carriers. 2+ The connection with NiCo spinel catalyst through oxygen bridge is beneficial to enhance the interaction between metal and support of Pd@NiCo spinel catalyst.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned Pd@NiCo spinel catalyst.

[0017] The design method of the present invention can exchange Pd atoms for Ni ion clusters in the NiCoPBA carrier with the assistance of a base to form Pd clusters and thermally derive them to form a spinel carrier with oxygen vacancies, and the steps are:

[0018] S1, preparing NiCoPBA carrier;

[0019] S1-1, dissolving NiCl2·6H2O and C6H5Na3O7 in ultrapure water to prepare system A; dissolving K3Co(CN)6 in ultrapure water to form system B; while maintaining stirring, adding system B into system A and mixing evenly, and then subjecting to aging treatment to obtain system C;

[0020] S1-2, washing and drying the system C prepared in S1-1 to obtain a NiCoPBA carrier;

[0021] Let n be the multiplication coefficient and n∈R + , then in S1-1:

[0022] In system A: the amount of NiCl2·6H2O added is n·[0.8242,4.121]g, the amount of C6H5Na3O7 added is n·[0.6,6]g, and the amount of ultrapure water added is n·[80,400]mL;

[0023] In system B: the amount of K3Co(CN)6 added was n·[0.532,5.32]g, and the amount of ultrapure water added was n·[80,400]mL;

[0024] S2, alkaline etching and ion exchange;

[0025] S2-1, adding the NiCoPBA carrier prepared in S1 and 1% Pd-loaded palladium acetylacetonate to ethanol, adding 5% ammonia water after ultrasonic dispersion, and continuously stirring to obtain system D;

[0026] S2-2, washing and drying the system D prepared in S2-1 to obtain Pd@NiCoPBA-N;

[0027] Let n be the multiplication coefficient and n∈R + , then in system D of S2-1: the amount of NiCoPBA added is n·[0.8,X]g, the amount of palladium acetylacetonate added is n·[0.001,0.1]g, and the amount of ammonia water added is n·[100,1000]mL;

[0028] Description: See Figure 1 , with the assistance of ammonia, the Ni in NiCoPBA(Ni3[Co(CN)6]2) was promoted 2+ The dissolution promoted the 2+ with Ni 2+ The ion exchange between NiCoPBA and Ni 2+ The highly ordered characteristics endow Pd with uniform dispersion on NiCoPBA, which in turn makes Pd in ​​the Pd@NiCo spinel catalyst highly dispersed, which is beneficial to the exposure of Pd active sites and promotes the activation of oxygen molecules to form active oxygen species. At the same time, the introduction of Pd into the NiCo spinel catalyst improves the mobility of lattice oxygen and produces a large number of oxygen vacancies, thereby improving the oxygen activation ability of the catalyst.

[0029] S3, support oxidation and Pd 2+ reduction;

[0030] S3-1, subjecting the Pd@NiCoPBA-N prepared in S2 to a pyrolysis treatment to obtain product A;

[0031] S3-2. The product A in S3-1 is subjected to secondary pyrolysis treatment to obtain a Pd@NiCo spinel catalyst.

[0032] Furthermore, the parameters of the primary pyrolysis treatment in S3-1 are: in an air atmosphere, the temperature is raised from room temperature to 300°C at a rate of 2-5°C / min, and kept at this temperature for 3h;

[0033] The parameters of the secondary pyrolysis treatment in S3-2 are: in a 10% H2 / Ar mixed atmosphere, the temperature is raised from room temperature to 200°C at a heating rate of 2-5°C / min and kept at this temperature for 2h.

[0034] Description: The above preparation method is based on the structural reversibility of NiCoPBA carrier and Ni 2+ The highly ordered characteristics of the clusters were effectively coupled with the advantages of ion exchange and MOFs derivatization to prepare Pd@NiCo spinel catalysts with highly dispersed Pd active sites and inherited NiCoPBA support morphology. 2+ The highly ordered Ni in the NiCoPBA support 2+ The exchange of clusters makes Pd 2+ The uniform embedding of NiCoPBA in the NiCo spinel catalyst effectively improves the mobility of active oxygen species and forms a large number of oxygen vacancies in situ, thereby significantly enhancing the oxygen activation ability of the Pd@NiCo spinel catalyst.

[0035] In a third aspect, the present invention provides an application of the above-mentioned Pd@NiCo spinel catalyst.

[0036] The Pd@NiCo spinel catalyst designed by the present invention based on the directional loading of PBA carrier can be applied to the degradation of VOCs, especially has a significant effect on the catalytic oxidation of toluene, and its mechanism of action is:

[0037] Toluene is adsorbed on the catalyst surface via π-π interactions and then ads and O latt The active oxygen species such as benzyl alcohol, benzaldehyde, benzoate and maleic anhydride are oxidized in sequence until they are completely oxidized to form harmless molecules such as CO2 and H2O. In the above reaction process, O2 molecules are captured by oxygen vacancies in the Pd@NiCo spinel catalyst and dissociated on the Pd active site. Part of the dissociated O2 is used to recombine the whole toluene and O latt The oxygen vacancies formed by the reaction can be converted into O adsDirectly participate in the catalytic oxidation process of toluene. Therefore, the Pd@NiCo spinel catalyst exposes more Pd active sites and has more oxygen vacancies and better lattice oxygen activity.

[0038] Compared with the existing PBA-based catalyst, the beneficial effects of the present invention are:

[0039] (1) The present invention is based on the structural reversible properties of NiCoPBA and Ni 2+ The highly ordered characteristics of the clusters effectively couple the advantages of ion exchange and MOFs derivatization to prepare Pd@NiCo spinel catalysts with highly dispersed Pd active sites and a NiCoPBA-like carrier morphology, providing a new research idea for the preparation of Pd@NiCo spinel catalysts with specific morphology and high dispersion of precious metals.

[0040] (2) The highly dispersed Pd active sites and NiCoPBA-like morphology of the Pd@NiCo spinel catalyst are conducive to promoting the dissociation of O2 molecules on the Pd active sites to form active oxygen species; at the same time, Pd is uniformly embedded in the NiCo spinel catalyst, which effectively improves the mobility of active oxygen species and forms a large number of oxygen vacancies in situ, thereby significantly improving the oxygen activation ability of the Pd@NiCo spinel catalyst. Therefore, the Pd@NiCo spinel catalyst prepared by the present invention exhibits excellent low-temperature activity and good stability in the catalytic oxidation of VOCs, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic diagram of the preparation principle of the Pd@NiCo spinel catalyst of the present invention;

[0042] Figure 2 : are SEM images of Pd@NiCo spinel catalysts; wherein, (a) is the SEM image of NiCoPBA, (b) is the SEM image of Pd@NiCoPBA, (c) is the SEM image of NiCo, and (d) is the SEM image of Pd@NiCo;

[0043] Figure 3 TEM images and element distribution maps of Pd@NiCo spinel catalysts; (a) is the HRTEM image of NiCo, (b) is the TEM image of Pd@NiCo, (d) is the HRTEM image of NiCo, (c), (e), (f) are the HRTEM images of Pd@NiCo, and (g) is the element distribution map of Pd@NiCo

[0044] Figure 4 The effect of different calcination temperatures on the Pd@NiCo spinel catalyst; (a) is the toluene conversion rate, (b) is the CO2 generation rate, toluene concentration: 1000ppm, space velocity 30000mL·g-1 ·h -1 ;

[0045] Figure 5 The effect of different reduction methods on Pd@NiCo spinel catalyst; (a) is the toluene conversion rate, (b) is the CO2 generation rate, toluene concentration: 1000ppm, space velocity 30000mL·g -1 ·h -1 ;

[0046] Figure 6 The effect of different H2 reduction temperatures on the Pd@NiCo spinel catalyst; (a) is the toluene conversion rate, (b) is the CO2 generation rate, toluene concentration: 1000ppm, space velocity 30000mL·g -1 ·h -1 ;

[0047] Figure 7 The effect of the preparation method on the catalyst is shown in Figure 1. (a) is the toluene conversion rate, (b) is the CO2 generation rate, toluene concentration: 1000ppm, space velocity 30000mL·g -1 ·h -1 ;

[0048] Figure 8 is the performance diagram of toluene catalyzed by different catalysts; where (a) is the toluene conversion rate, (b) is E a , (c) is r, (d) is r s , toluene concentration: 1000ppm, space velocity 30000mL·g -1 ·h -1 ;

[0049] Fig. 9 The Pd@NiCo spinel catalyst has different space velocity (toluene concentration is fixed at 1000ppm) and concentration (space velocity is fixed at 30000mL·g -1 ·h -1 ) (Toluene concentration: 1000ppm, 5vol% water vapor, space velocity 30000mL·g -1 ·h -1 );

[0050] Fig.10 The performance diagram of toluene catalyzed by different catalysts; (a) is the conversion rate diagram of toluene by NiCo catalyst and Pd@NiCo spinel catalyst, and (b) is the generation rate diagram of CO2 by NiCo catalyst and Pd@NiCo spinel catalyst;

[0051] Fig.11The hydrothermal stability diagram of Pd@NiCo spinel catalyst at 230°C; (a) is the hydrostability; (b) is the thermal stability, toluene concentration: 1000ppm, 5vol% water vapor, space velocity 30000mL·g -1 ·h -1 ;

[0052] Fig.12 are XRD spectra of different catalysts; (a) is the XRD spectra of catalysts NiCoPBA, NiCoPBA-N, and PdCoPBA-N, and (b) is the XRD spectra of catalysts NiCo, NiCo-N, and Pd@NiCo;

[0053] Fig.13 The N2 adsorption-desorption isotherms and pore size distribution diagrams of different catalysts; (a) is the N2 adsorption-desorption isotherms of NiCo, Pd / NiCo, and Pd@NiCo catalysts, and (b) is the pore size distribution diagram of NiCo, Pd / NiCo, and Pd@NiCo catalysts;

[0054] Fig.14 These are the EPR spectra of different catalysts. DETAILED DESCRIPTION

[0055] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0056] Example 1: This example describes a Pd@NiCo spinel catalyst, the content of which is as follows.

[0057] The present invention designs a Pd@NiCo spinel catalyst based on a PBA carrier directional loading, which has a periodic structure with complete functions including:

[0058] Spinel, which inherits the microstructure of PBA support and has oxygen vacancies, and metal clusters connected to the spinel support through oxygen bridges;

[0059] There is a strong metal-support interaction between the metal clusters and the spinel;

[0060] The PBA carrier is a NiCoPBA carrier; the metal cluster is a Pd cluster, and its particle size ranges from 1 to 20 nm; the spinel is a NiCo spinel;

[0061] Generally speaking, strong metal-support interaction refers to the strong electronic and geometric interactions between metal catalysts and their supports, which can significantly change the electronic properties and morphology of the catalysts, thereby affecting their catalytic performance. In this case, it refers to the significant electronic interactions between Pd clusters and NiCoPBA supports.

[0062] The surface area of ​​the Pd@NiCo spinel catalyst is 134.6 m 2 / g, the average pore size is 0.28cm 3 / g, and the average pore size is 17.92nm.

[0063] Example 2: This example describes a method for preparing the Pd@NiCo spinel catalyst in Example 1, the content of which is as follows.

[0064] S1, preparing NiCoPBA carrier;

[0065] S1-1, dissolve NiCl2·6H2O and C6H5Na3O7 in ultrapure water to prepare system A; dissolve K3Co(CN)6 in ultrapure water to form system B; keep stirring, add system B into system A and mix evenly for 30 minutes, then age for 24 hours to obtain system C;

[0066] In system A: the amount of NiCl2·6H2O added is 0.8242 g, the amount of C6H5Na3O7 added is 0.6 g, and the amount of ultrapure water added is 80 mL;

[0067] In system B: the amount of K3Co(CN)6 added was 0.532 g, and the amount of ultrapure water added was 80 mL;

[0068] S1-2, washing the system C prepared in S1-1 with ultrapure water and ethanol alternately, and drying the system C to obtain a NiCoPBA carrier;

[0069] S2, alkaline etching and ion exchange;

[0070] S2-1, adding the NiCoPBA carrier prepared in S1 and 1% Pd-loaded palladium acetylacetonate to ethanol, adding 5% ammonia water after ultrasonic dispersion, and continuously stirring to obtain system D;

[0071] In system D: the amount of NiCoPBA added was 0.8 g, the amount of palladium acetylacetonate added was 0.0001 g, and the amount of ammonia water added was 100 mL;

[0072] S2-2, washing and drying the system D prepared in S2-1 to obtain Pd@NiCoPBA-N;

[0073] S3, support oxidation and Pd 2+ reduction;

[0074] S3-1, subjecting the Pd@NiCoPBA-N prepared in S2 to a pyrolysis treatment to obtain product A;

[0075] The parameters of the primary pyrolysis treatment were as follows: in air atmosphere, the temperature was raised from room temperature to 300 °C at a rate of 2 °C / min and kept at this temperature for 3 h;

[0076] S3-2, subjecting the product A in S3-1 to secondary pyrolysis to obtain a Pd@NiCo spinel catalyst;

[0077] The parameters of the secondary pyrolysis treatment are: in a 10% H2 / Ar mixed atmosphere, the temperature is increased from room temperature to 200°C at a heating rate of 2°C / min and kept at this temperature for 2h.

[0078] Example 3: The contents of this example are based on Example 2, and are intended to illustrate the preparation method of Pd@NiCo spinel catalyst under another parameter. Except for the following contents, the rest are the same.

[0079] S2, alkaline etching and ion exchange;

[0080] S2-1, adding the NiCoPBA carrier prepared in S1 and 1% Pd-loaded palladium acetylacetonate to ethanol, adding 5% ammonia water after ultrasonic dispersion, and continuously stirring to obtain system D;

[0081] In system D: the amount of NiCoPBA added was 0.8 g, the amount of palladium acetylacetonate added was 0.008 g, and the amount of ammonia water added was 100 mL;

[0082] S2-2, washing and drying the system D prepared in S2-1 to obtain Pd@NiCoPBA-N;

[0083] Example 4: The content of this example is based on Example 2, and is intended to illustrate the preparation method of Pd@NiCo spinel catalyst under another parameter. The content is as follows.

[0084] S1, preparing NiCoPBA carrier;

[0085] S1-1, dissolve NiCl2·6H2O and C6H5Na3O7 in ultrapure water to prepare system A; dissolve K3Co(CN)6 in ultrapure water to form system B; keep stirring, add system B into system A and mix evenly for 30 minutes, then age for 24 hours to obtain system C;

[0086] In system A: the amount of NiCl2·6H2O added is 4.121 g, the amount of C6H5Na3O7 added is 6 g, and the amount of ultrapure water added is 400 mL;

[0087] In system B: the amount of K3Co(CN)6 added was 5.32 g, and the amount of ultrapure water added was 400 mL;

[0088] S1-2, washing the system C prepared in S1-1 with ultrapure water and ethanol alternately, and drying the system C to obtain a NiCoPBA carrier;

[0089] S2, alkaline etching and ion exchange;

[0090] S2-1, adding the NiCoPBA carrier prepared in S1 and 1% Pd-loaded palladium acetylacetonate to ethanol, adding 5% ammonia water after ultrasonic dispersion, and continuously stirring to obtain system D;

[0091] In system D: the amount of NiCoPBA added is 8 g, the amount of palladium acetylacetonate added is 0.1 g, and the amount of ammonia water added is 1000 mL;

[0092] S2-2, washing and drying the system D prepared in S2-1 to obtain Pd@NiCoPBA-N;

[0093] S3, support oxidation and Pd 2+ reduction;

[0094] S3-1, subjecting the Pd@NiCoPBA-N prepared in S2 to a pyrolysis treatment to obtain product A;

[0095] The parameters of the primary pyrolysis treatment were as follows: in air atmosphere, the temperature was raised from room temperature to 300 °C at a rate of 5 °C / min and kept at this temperature for 3 h;

[0096] S3-2, subjecting the product A in S3-1 to secondary pyrolysis to obtain a Pd@NiCo spinel catalyst;

[0097] The parameters of the secondary pyrolysis treatment are: in a 10% H2 / Ar mixed atmosphere, the temperature is increased from room temperature to 200°C at a heating rate of 5°C / min and kept at this temperature for 2h.

[0098] Comparative Example 1: This comparative example is intended to illustrate the preparation method of Pd-loaded NiCo spinel catalyst (i.e., Pd / NiCo-L catalyst) prepared by a grinding method. Except for the following contents, the rest of the preparation method is the same as Example 2.

[0099] 0.8 g of NiCoPBA and 0.008 g of 1% Pd-loaded palladium acetylacetonate were thoroughly ground and mixed, and then pyrolyzed under the following conditions to obtain Pd / NiCo-L.

[0100] Pyrolysis parameters: in air atmosphere, heat up to 300°C at a heating rate of 2°C / min and keep warm for 3h.

[0101] Comparative Example 2: This comparative example is intended to illustrate the preparation method of Pd-loaded NiCo spinel catalyst (i.e., Pd / NiCo catalyst) prepared by a hydrothermal method. Except for the following contents, the rest of the preparation method is the same as Example 2.

[0102] Take 0.8 g of NiCoPBA and 0.008 g of 1% Pd-loaded acetylacetonate palladium and dissolve them in 100 mL of ultrapure water. Then heat the mixture at 100° C. until the water evaporates. After the crystallized product is dried in an oven, it is thermally decomposed under the following conditions to obtain Pd / NiCo.

[0103] Comparative Example 3: This comparative example is intended to illustrate the preparation method of a NiCo spinel catalyst (i.e., NiCoPBA-N catalyst) without Pd loading. Except for the following contents, the rest of the preparation method is the same as that of Example 2.

[0104] 0.8 g of NiCoPBA carrier was added to ethanol, and after ultrasonic dispersion for 15 min, 100 mL of 5% ammonia water was added and stirred for 1 h.

[0105] After stirring, the product is washed alternately with ultrapure water and ethanol, and the washed product is placed in an oven for drying to obtain NiCoPBA-N.

[0106] Experimental example: The description of this experimental example is based on the recorded schemes in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 2, and is intended to illustrate the practical application effect of the present invention.

[0107] 1. Experimental parameter optimization

[0108] 1-1. Optimization of ammonia concentration

[0109] Table 1 ICP test results of Pd@NiCo spinel catalysts synthesized at different ammonia concentrations

[0110]

[0111] Ammonia is the key to the construction of Pd@spinel catalysts derived from MOFs by alkali-assisted ion exchange coupling. Therefore, the effect of ammonia concentration on NiCoPBA was investigated. Table 1 shows the ICP test results of Pd@NiCo spinel catalysts under different ammonia concentrations. It can be seen from the last row of the table that no Pd loading was detected in the catalyst when water was added. Compared with the Pd loading detected after adding ammonia, the results show that the effective loading of Pd cannot be achieved by NiCoPBA adsorption alone; further analysis of the fourth and fifth columns of the table shows that the Pd loading in the Pd@NiCo spinel catalyst increases with the decrease of Ni / Co molar ratio, which verifies the synthesis mechanism of Pd exchanging Ni; when the ammonia concentration is between 0-5%, the Pd loading increases with the increase of ammonia concentration, and between 5%-10%, the Pd loading decreases with the increase of ammonia concentration, indicating that too high ammonia concentration will cause the PBA skeleton to be dissolved, resulting in a decrease in loading or Pd dissolution. Therefore, an ammonia concentration of 5% was selected as the optimization condition in subsequent experiments.

[0112] 1-2. Optimization of roasting temperature

[0113] The calcination temperature affects the energy consumption and performance of MOFs-derived catalysts. The principle is to keep the temperature as low as possible when the performance is optimal. Figure 4 As shown, T 90% The performance trend is 300℃<350℃<400℃<250℃, and the CO2 generation rate also shows the same trend. Based on this, we choose 300℃ as the calcination temperature of the catalyst in subsequent experiments.

[0114] 1-3. Optimization of restoration method

[0115] The reduction method is also a key factor in the performance of precious metal catalysts. Based on this, we investigated the effects of H2 reduction and sodium borohydride reduction on the catalyst performance. Figure 5 It can be seen that the performance of the catalysts after reduction was significantly improved. Among them, the performance of the catalysts using the H2 reduction method increased from the original T 90% =245℃ was reduced to 231℃, which is better than the sodium borohydride reduction method. This is because the H2 reduction method can obtain smaller Pd particles in the reduction of chemically anchored dispersed Pd-based metal sources and exhibit better low-temperature activity compared to the sodium borohydride reduction method. In addition, the H2 reduction method also has small sample loss during the operation process and is easy to control the precious metals from being re-oxidized after reduction, making it one of the mainstream processes for preparing precious metal catalysts for catalytic oxidation of VOCs. Therefore, subsequent experiments all used the H2 reduction method to further improve the catalyst.

[0116] 1-4. Optimization of different H2 reduction temperatures

[0117] See also Figure 6, temperature is a key factor affecting hydrogen reduction. At low temperatures, the reaction rate is low; as the temperature rises, the reaction rate accelerates and the hydrogen reduction curve rises. High temperature is conducive to overcoming the activation energy of the reaction, thereby promoting the reaction, but too high a temperature can easily cause Pd to be excessively reduced to form PdO, which in turn reduces the performance. Based on this, choosing a suitable hydrogen reduction temperature is crucial to optimizing catalyst performance. The trend of the catalytic oxidation of toluene T90% at different reduction temperatures is 200℃<150℃<250℃<300℃, and the CO2 generation rate also shows the same trend. Therefore, the H2 reduction temperature for subsequent experiments is selected at 200℃.

[0118] 2. Performance experiment of catalytic oxidation of toluene over Pd@NiCo spinel catalyst

[0119] 2-1. Comparison of different preparation methods

[0120] Table 2 ICP test results of PdCo-N prepared by different methods

[0121]

[0122] In order to verify the superiority of the ammonia-assisted ion exchange coupling MOFs derivatization method, the Pd-loaded NiCo spinel catalyst with the same Pd loading was prepared by the traditional method (grinding method and hydrothermal synthesis method). The test results are shown in Figure 2. Figure 7 As shown in Table 2. It can be clearly seen from the figure that the catalyst performance prepared by the ammonia-assisted ion exchange coupling MOFs derivatization method is significantly better than that of the hydrothermal synthesis method and the grinding method. 90% It is 228℃, which is better than the hydrothermal method (248℃) and the grinding method (255℃).

[0123] 2-2. Intrinsic activity experiment

[0124] Table 3 Performance of different catalysts

[0125]

[0126] Note: The reaction temperature was 160°C.

[0127] In order to further obtain the intrinsic activity of the catalyst constructed by the ammonia-assisted ion exchange coupling MOFs derivatization method, we conducted a series of kinetic experiments on three catalysts: NiCo, Pd / NiCo, and Pd@NiCo. Figure 8As shown in Table 3, the apparent activation energy of the Pd@NiCo spinel catalyst is 43.2 kJ / mol, which is much lower than that of NiCo (139.8 kJ / mol) and Pd / NiCo (57.4 kJ / mol) catalysts, indicating that the ammonia-assisted ion exchange coupled MOFs-derived Pd@NiCo spinel catalyst has the best low-temperature catalytic oxidation activity for toluene.

[0128] Further observation Figure 8 (c) and Table 3 show that the Pd@NiCo spinel catalyst has the highest reaction rate at three different low temperatures of 155℃, 160℃, and 165℃, further proving that its low-temperature activity is the best. Generally, the activity of a catalyst is closely related to its specific surface area. Generally speaking, the specific surface area affects the exposure of active sites, so we attribute the good catalytic performance of a catalyst to its large specific surface area. Therefore, we normalized the reaction rate by BET specific surface area, and the results are shown in Figure 8 (d) As shown in Table 3, after BET surface area normalization treatment, the Pd@NiCo spinel catalyst still has the highest reaction rate at three different low temperatures of 155°C, 160°C, and 165°C, indicating that in addition to the key factor of specific surface area, there are also key factors that affect the catalytic oxidation performance of toluene by Pd@NiCo spinel catalyst.

[0129] 2-3. Performance of Pd@NiCo spinel catalyst at different space velocity concentrations

[0130] The space velocity and concentration of the exhaust gas generated in actual working conditions are constantly changing. Based on this, we explored the performance of Pd@NiCo spinel catalyst under different space velocity concentrations. The test results are as follows: Fig. 9 As shown, Fig. 9 (a) 5000 mL·g -1 ·h -1 、10000mL·g -1 ·h -1 , 20000mL·g -1 ·h -1 The catalytic oxidation performance of toluene by Pd@NiCo spinel catalyst under space velocity conditions. We found that with the increase of space velocity, the catalyst performance showed a downward trend. This may be because with the increase of space velocity, the contact time between pollutants and catalysts decreased, which was not conducive to the catalyst adsorption of toluene. Fig. 9 (b) is the catalytic oxidation performance curve of Pd@NiCo spinel catalyst at toluene concentrations of 500ppm, 1000ppm, and 2000ppm. Analysis shows that with the increase of pollutant concentration, the catalyst performance also shows a downward trend. This is because the total amount of pollutants on the catalyst surface increases per unit time, so the catalyst requires a higher temperature to oxidize the pollutants on its surface.

[0131] 2-4. Catalytic performance test under water vapor

[0132] Since the VOCs gas generated in actual industrial applications inevitably contains a certain amount of water vapor, in order to better simulate the actual industrial application scenario, we further tested the NiCo and Pd@NiCo spinel catalysts under the condition of adding 5 vol% water vapor. Fig.10 As shown in Figure 2, the Pd@NiCo spinel catalyst can still maintain stable and good low-temperature activity under the condition of adding 5 vol% water vapor, and its T 90 , T 50 , T 20 They are 229℃, 217℃, and 205℃ respectively. The test results are Figure 8 They are basically consistent, indicating that the catalysts regulated by the system in this chapter can achieve good results in industrial practice and have good application prospects.

[0133] 2-5. Stability performance test

[0134] Stability is also an important indicator of catalytic performance, so it is necessary to test the hydrothermal stability of the catalyst. Fig.11 Pd@NiCo spinel catalyst at 230℃, toluene concentration of 1000ppm, 5vol% water vapor, space velocity of 30000mL·g -1 ·h -1 The hydrothermal stability test was carried out for 30 hours under the conditions. During the whole experiment, the toluene conversion rate remained stable without obvious decline. After the introduction of water vapor, the toluene conversion rate remained above 90%, which shows that the Pd@NiCo spinel catalyst has good hydrothermal stability, which lays the foundation for its practical application.

[0135] 3. Structural characterization and structure-activity relationship of Pd@NiCo spinel catalyst

[0136] 3-1. XRD characterization

[0137] The crystal structure of the catalyst was characterized by XRD technique. Fig.12 (a) is the XRD spectra of NiCoPBA, NiCoPBA-N, and PdCoPBA-N. As can be seen from the figure, the three catalysts all have a series of diffraction peaks at 2θ=17.4, 25.8, 36.8, and 43.1°, which correspond to the characteristic peaks of NiCo composite oxides. This shows that the catalyst after the alkaline etching ion exchange system still inherits the template of the precursor. Fig.12(b) is the XRD spectra of NiCo, NiCo-N, and Pd@NiCo. Analysis shows that the three catalysts all have a series of diffraction peaks at 2θ=38.1, 44.2°, and 64.5, which correspond to the characteristic peaks of NiCo spinel catalysts. This result proves that the catalyst successfully converts NiCoPBA into NiCo spinel catalyst at a calcination temperature of 300°C. It also shows that the calcination temperature of 300°C will not affect the intrinsic structure of the catalyst. The above analysis results also lay the foundation for the subsequent structure-activity relationship analysis.

[0138] 3-2. SEM characterization

[0139] Figure 2 This is the SEM image of the catalyst. It can be found that the catalyst after the ammonia exchange system still inherits the template of NiCoPBA and is cubic in shape. This structure is conducive to fully exposing the active sites in the catalyst, thereby improving the low-temperature activity.

[0140] 3-3. TEM characterization and element distribution characterization

[0141] Figure 3 (a) and (b) are TEM images of NiCo and Pd@NiCo spinel catalysts. It can be seen from the figure that both NiCo and Pd@NiCo have cubic morphology, indicating that the catalysts after alkaline etching and ion exchange system still inherit the template of the precursor very well, which is consistent with the SEM analysis results. In addition, the fine structure of NiCo and Pd@NiCo catalysts was characterized by HRTEM technology. Figure 3 (d) and (e) show that both catalysts have lattice fringes with a spacing of about 0.285 nm, which corresponds to the (220) crystal plane of the NiCo spinel catalyst. This result further proves that the catalyst was successfully converted from NiCoPBA to NiCo spinel catalyst after alkaline etching and ion exchange and calcination at 300 ° C. In addition, the presence of Pd atoms can be clearly seen in the red box points in 3 (c) and (f), indicating that Pd was successfully loaded on the NiCo spinel catalyst. Figure 3 (g) is the element distribution diagram of Pd@NiCo spinel catalyst, from which it can be seen that Ni, Co, O, and Pd elements are evenly distributed.

[0142] 3-4. Catalyst pore size distribution and specific surface area characterization

[0143] Table 4 Catalyst pore structure information

[0144]

[0145] In order to characterize the pore size distribution and specific surface area of ​​the catalyst, we used a fully automatic physical microporous adsorption instrument to test the N2 adsorption / desorption of three catalysts: NiCo, Pd / NiCo, and Pd@NiCo. The test results are shown in Figure 2. Fig.13 As shown, Fig.13 Table 4 is the N2 adsorption / desorption isotherm results of the catalysts, and Table 5 is the summary of the pore structure information corresponding to the three catalysts. Fig.13 (a) It can be seen that the N2 adsorption / desorption isotherms of the three catalysts NiCo, Pd / NiCo, and Pd@NiCo are all typical type IV isotherms with H2-type hysteresis loops, indicating that the three catalysts all have the characteristics of mesoporous structures. This result is further demonstrated in the BJH pore size distribution diagram. From the summary of the pore structure information, it can be concluded that the specific surface areas S of the three catalysts are BET The size order is Pd@NiCo(134.6m 2 / g)>Pd / NiCo(115.9m 2 / g)>NiCo(77.23m 2 / g). The average pore volume V is ranked as follows: Pd@NiCo (0.28 cm 3 / g)>Pd / NiCo(0.22cm 3 / g)>NiCo(0.17cm 3 / g). The order of average pore size D is Pd / NiCo (22.21nm)>NiCo (17.98nm)>Pd@NiCo (17.92nm). The analysis results show that the specific surface area and pore volume of the catalyst are increased under the ammonia-assisted ion exchange system, making the pore structure richer. The rich pore structure can reduce the mass transfer resistance during the catalytic oxidation process, promote the contact between toluene and active sites during the reaction, help the mass transfer of pollutants, and improve the catalytic oxidation efficiency. This is one of the reasons why the Pd@NiCo spinel catalyst has a better low-temperature catalytic oxidation performance of toluene.

[0146] 3-5. EPR characterization

[0147] Fig.14 The electron paramagnetic resonance spectra of three catalysts NiCo, Pd / NiCo, and Pd@NiCo are shown in the figure. As can be seen from the figure, each catalyst has a symmetrical EPR signal peak at g=2.003, indicating that there are certain concentrations of oxygen vacancies in the three catalysts. Further analysis shows that the signal peak of the Pd@NiCo spinel catalyst is the strongest, followed by Pd / NiCo and NiCo, which indicates that the oxygen vacancy concentration of the catalyst has been improved after the ammonia exchange system. The EPR analysis results are also consistent with the above XPS analysis results.

[0148] Based on the above analysis, the synergistic effect of precious metal Pd active sites and oxygen vacancy active sites on the catalyst is the fundamental reason why the Pd@NiCo spinel catalyst has excellent catalytic performance.

Claims

1. A Pd@NiCo spinel catalyst based on a PBA carrier directional loading, characterized in that: The Pd@NiCo spinel catalyst has a periodic structure with complete functions including: Spinel, which inherits the microstructure of PBA support and has oxygen vacancies, and metal clusters connected to the spinel support through oxygen bridges; There is a strong metal-support interaction between the metal cluster and the spinel; The PBA carrier is a NiCoPBA carrier; the metal cluster is a Pd cluster, and its particle size ranges from 1 to 20 nm; the spinel is a NiCo spinel; The surface area of ​​the Pd@NiCo spinel catalyst is 134.6 m 2 / g, the average pore size is 0.28cm 3 / g, and the average pore size is 17.92nm.

2. The method for preparing a Pd@NiCo spinel catalyst based on a directional loading of a PBA carrier according to claim 1, characterized in that: Base-assisted formation of highly ordered Ni in NiCoPBA supports 2+ Cluster and Pd 2+ Exchange, so that Pd 2+ Evenly dispersed on the NiCoPBA support, Pd 2+ The reduction process forms a highly dispersed Pd active site, thereby obtaining a Pd@NiCo spinel catalyst that inherits the morphology of the NiCoPBA support. The specific steps are as follows: S1, preparing NiCoPBA carrier; S1-1, dissolving NiCl2·6H2O and C6H5Na3O7 in ultrapure water to prepare system A; dissolving K3Co(CN)6 in ultrapure water to form system B; while maintaining stirring, adding system B into system A and mixing evenly, and then subjecting to aging treatment to obtain system C; S1-2, washing and drying the system C prepared in S1-1 to obtain a NiCoPBA carrier; Let n be the multiplication coefficient and n∈R + , then in S1-1: In system A: the amount of NiCl2·6H2O added is n·[0.8242,4.121]g, the amount of C6H5Na3O7 added is n·[0.6,6]g, and the amount of ultrapure water added is n·[80,400]mL; In system B: the amount of K3Co(CN)6 added was n·[0.532,5.32]g, and the amount of ultrapure water added was n·[80,400]mL; S2, alkaline etching and ion exchange; S2-1, adding the NiCoPBA carrier prepared in S1 and 1% Pd-loaded palladium acetylacetonate to ethanol, adding 5% ammonia water after ultrasonic dispersion, and continuously stirring to obtain system D; S2-2, washing and drying the system D prepared in S2-1 to obtain Pd@NiCoPBA-N; Let n be the multiplication coefficient and n∈R + , then in the system D of S2-1: the amount of NiCoPBA added is n·[0.8,8]g, the amount of palladium acetylacetonate added is n·[0.0001,0.1]g, and the amount of ammonia water added is n·[100,1000]mL; S3, support oxidation and Pd 2+ reduction; S3-1, subjecting the Pd@NiCoPBA-N prepared in S2 to a pyrolysis treatment to obtain product A; S3-2. The product A in S3-1 is subjected to secondary pyrolysis treatment to obtain a Pd@NiCo spinel catalyst.

3. The method for preparing a Pd@NiCo spinel catalyst based on a directional loading of a PBA carrier according to claim 2, characterized in that: The parameters of the primary pyrolysis treatment in S3-1 are: in an air atmosphere, the temperature is raised from room temperature to 300°C at a rate of 2-5°C / min, and kept at this temperature for 3 hours; The parameters of the secondary pyrolysis treatment in S3-2 are: in a 10% H2 / Ar mixed atmosphere, the temperature is raised from room temperature to 200°C at a heating rate of 2-5°C / min and kept at this temperature for 2h.

4. Application of Pd@NiCo spinel catalyst based on PBA carrier directional loading in catalytic oxidation of VOCs.

Citation Information

Patent Citations

  • Simple synthesis method for adjusting morphology of spinel or prussian blue nanometer material

    CN108217691A

  • Preparation method of controllable etching MOFs (Metal-Organic Frameworks) derived low-temperature efficient doped VOCs (Volatile Organic Compounds) catalyst

    CN115069264A

  • Spinel CeO2 catalyst as well as preparation method and application thereof

    CN117065760A

  • Prussian blue derived catalysts

    US20200261893A1