Preparation method of flame-retardant particle artificial board
Through plasma surface treatment technology, the flame retardant polymerization reaction of wood particulate materials is stimulated, combined with spraying adhesives, the problems of flame retardant and glue strength of particulate artificial boards are solved, and the high-efficiency flame retardant and mechanical strength are improved, adapting to the existing Production process.
Patent Information
- Application Number
- CN202411266280.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
AI Technical Summary
In the flame retardant treatment, existing particulate artificial boards have problems such as long drying time, high cost, and easy to lead to curling and deterioration of adhesive strength. Commonly used flame retardants have a great impact on the curing of adhesives and affect the hot pressing process.
Plasma surface treatment technology is used to stimulate the polymerization reaction of water-soluble flame retardant on the surface of wood particulate materials, forming a stable polymer network, increasing the combination of flame retardant and wood particulate materials, and promoting the spraying of adhesives and flame retardants Adhesive spread to improve mechanical meshing effect.
The flame retardant effect and mechanical strength of particulate artificial boards have been significantly improved, with the ultimate hydrogen index (LOI) reaching 33%-45%, and the static curved strength is as high as 10.5MPa-15.7MPa, which meets relevant standards and does not affect the existing production process.
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the flame retardancy and bonding performance of particle artificial boards by utilizing plasma surface treatment technology and flame retardants, and belongs to the field of artificial board manufacturing. Background Art
[0002] Particle board is a type of man-made board made by cutting various branches, small-diameter wood, sawdust, etc. into shavings or fibers, then applying adhesives, paving, pre-pressing and hot-pressing. The most common ones are particleboard and fiberboard. As global wood stocks decrease, the market demand for particle board has increased year by year. As of December 31, 2020, the global annual production capacity of particleboard was 114.3 million cubic meters. However, due to the high amount of glue applied to particle board, it is a combustible material and is prone to fire. According to the national standard GB20286-2006 "Combustion Performance Requirements and Labeling of Flame-retardant Products and Components in Public Places", particle boards entering public places must have the corresponding flame retardant performance level. The commonly used flame retardant treatment methods are the following two methods:
[0003] 1. Impregnation of wood particle materials. Impregnate wood particle materials in water-soluble flame retardant or small molecule flame retardant solution, and infiltrate the flame retardant into the wood particle materials through osmotic pressure. This method requires secondary drying, which takes a long time and is costly. Drying after impregnation can easily cause the shavings or fibers to curl, affecting paving.
[0004] 2. Flame retardant fillers. Adding powder or liquid flame retardants during the gluing process is simple to operate and the flame retardant is evenly distributed, but flame retardants with obvious acidity and alkalinity will affect the curing of the adhesive and the hot pressing process; adding a large amount of powdered flame retardants will cause a significant decrease in the bonding strength of the particleboard.
[0006] To this end, the present invention uses plasma technology to stimulate the polymerization reaction of the water-soluble flame retardant on the surface of the wood particle material to form a stable polymer network. When the plasma contains a large number of high-energy active particles such as electrons, ions and free radicals and contacts the flame retardant molecules on the surface of the wood particle material, it can trigger its polymerization reaction, thereby enhancing the binding effect between the flame retardant and the wood particle material. At the same time, the plasma treatment promotes the spreading of the adhesive on the surface of the wood particle material, thereby increasing the contact area between the adhesive and the wood particle material and forming a good mechanical meshing effect. The bonding strength of the artificial board is improved. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a method for preparing a flame retardant particle artificial board to solve the problems raised in the above background technology.
[0008] To achieve the above object, the present invention provides the following technical solution: a method for preparing a flame retardant particle board, comprising the following steps: A method for preparing a flame retardant particle board comprises the following steps: S1. Weigh wood particles such as wood shavings and fibers, spray the surface with a flame retardant solution, and then dry it until the moisture content is stabilized at 2-5%. The amount of flame retardant added is 5-20% of the mass of the absolutely dry wood particles. S2, performing plasma treatment on the wood particulate material after step S1; S3. Add adhesive and flame retardant to the wood particle material after plasma treatment by spraying, stir evenly, and apply adhesive in an amount of 5-20% of the mass of the absolutely dry wood particle material. Perform paving, pre-pressing, hot pressing, trimming, sanding and other treatments to obtain flame-retardant particle artificial board.
[0009] The selected plasma discharge structure is one of dielectric barrier discharge, radio frequency discharge, atmospheric jet discharge, and microwave discharge; the discharge power is 0.1-6kW; the discharge atmosphere is one or more of nitrogen, oxygen, air, and argon, and the discharge time is 3-20s.
[0010] The adhesive is selected from urea-formaldehyde resin, melamine resin, phenolic resin and isocyanate adhesive.
[0011] The method for preparing a flame-retardant particle artificial board is characterized in that the composite flame retardant in step S1 includes the following components: a solution of one or more of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, boric acid, borax, phytic acid, diammonium phosphate, ammonium polyphosphate, guanyl phosphate urea, hydroxyethylenediphosphonic acid, potassium salt of hexadecanol phosphate, and bis(4-hydroxyphenyl)phenylphosphine oxide.
[0013] Compared with the prior art, the present invention has the following beneficial effects: (1) Significant flame retardant effect: Plasma contains a large number of high-energy active particles such as electrons, ions and free radicals. When they come into contact with the flame retardant molecules on the surface of the wood particle material, a polymerization reaction is initiated, allowing the flame retardant to penetrate and fix better in the wood particle material. When the flame retardant addition amount is only 5-20%, the limiting hydrogen index (LOI) of the particleboard prepared is as high as 33%-45%, and the limiting hydrogen index (LOI) of the fiberboard prepared is as high as 32%-40%, achieving high flame retardancy. (2) Enhance the mechanical strength of artificial boards: Plasma treatment promotes the spreading of adhesives, increases the contact area between adhesives and wood particles, forms good mechanical meshing, and improves the bonding strength of artificial boards. The flame-retardant particleboard prepared by this method has a static bending strength of up to 10.5MPa-15.7MPa, which meets the standard static bending strength (11MPa) required for load-bearing particleboards in a dry state specified in GBT 4897-2015 "Particleboard". The flame-retardant fiberboard prepared by this method has a limiting hydrogen index (LOI) of up to 32%-40% and a static bending strength of up to 23MPa-29MPa, which meets the standard static bending strength (24MPa) required for load-bearing particleboards in a dry state specified in GB / T 11718-2009 "Medium Density Fiberboard and Density Fiberboard".
[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Specific embodiments In the following implementation examples, the wood particle material is selected from poplar wood shavings with a thickness of about 0.5 mm or poplar wood fibers with a length of about 40 mm.
[0016] Control group 1: Weigh wood particles such as wood shavings and fibers, spray borax flame retardant solution on their surface, the amount of flame retardant added is 20% of the absolute dry wood shavings / fibers, then dry the wood shavings / fibers to balance their moisture content at 4%; add urea-formaldehyde resin adhesive to the wood shavings / fibers by spraying, stir evenly, and the amount of adhesive applied is 20% of the wood shavings / fibers. The wood shavings / fibers after mixing with adhesive are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood shavings / fiberboard.
[0017] The performance test of the control group 1 showed that the limiting oxygen index of the particleboard was 31.8%, and the static bending strength was 8.8MPa. The limiting oxygen index of the fiberboard was 31.8%, and the static bending strength was 23.1MPa.
[0018] Control group 2: Weigh wood particles such as wood shavings and fibers, dry the shavings / fibers, and balance their moisture content to 4%; then use dielectric barrier discharge plasma to treat the surface of the shavings / fibers, with a treatment power of 4.5kW and air as the treatment atmosphere; add urea-formaldehyde resin adhesive to the shavings by spraying, stir evenly, and apply 20% of the mass of the absolutely dry shavings / fibers. The shavings / fibers after adhesive application are paved, pre-pressed, hot-pressed, trimmed, sanded, etc. to obtain flame-retardant shavings / fiberboard.
[0019] The performance test of control group 2 showed that the limiting oxygen index of particleboard was 24.1%, and the static bending strength was 22.5MPa. The limiting oxygen index of flame retardant fiberboard was 22.8%, and the static bending strength was 28.8MPa.
[0020] Example 1: Weigh wood particles such as wood chips and fibers, spray 1,3,5-tris(2-hydroxyethyl)cyanuric acid flame retardant solution on the surface, and the amount of flame retardant added is 5% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use dielectric barrier discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 4.5kW, and the treatment atmosphere is air; urea-formaldehyde resin adhesive is added to the wood chips / fibers by spraying, stirred evenly, and the amount of glue applied is 5% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0021] Embodiment 1 Performance test shows that the limiting oxygen index of the flame retardant particle board is 33.3%, and the static bending strength is 10.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 32.8%, and the static bending strength is 27.2 MPa.
[0022] Example 2: Weigh wood particles such as wood chips and fibers, spray a boric acid flame retardant solution on their surface, and the amount of flame retardant added is 5% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use dielectric barrier discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 8kW, and the treatment atmosphere is air; add urea-formaldehyde resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 5% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot-pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0023] The performance test of Example 2 shows that the limiting oxygen index of the flame retardant particle board is 40.3%, and the static bending strength is 13.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 36.8%, and the static bending strength is 27.8 MPa.
[0024] Example 3: Weigh wood particles such as wood chips and fibers, spray a borax flame retardant solution on their surface, and the amount of flame retardant added is 20% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use dielectric barrier discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 8kW, and the treatment atmosphere is air; add urea-formaldehyde resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 20% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot-pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0025] The performance test of Example 3 shows that the limiting oxygen index of the flame retardant particle board is 42.4%, and the static bending strength is 15.7 MPa. The limiting oxygen index of the flame retardant fiberboard is 37.5%, and the static bending strength is 27.5 MPa.
[0026] Example 4: Weigh wood particles such as wood chips and fibers, spray a phytic acid flame retardant solution on their surface, and the amount of flame retardant added is 5% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use atmospheric jet discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 4.5kW, and the treatment atmosphere is nitrogen; add melamine urea-formaldehyde resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 5% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0027] The performance test of Example 4 shows that the limiting oxygen index of the flame retardant particle board is 35.3%, and the static bending strength is 11.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 31.8%, and the static bending strength is 28.8 MPa.
[0028] Example 5: Weigh wood particles such as wood chips and fibers, spray a diammonium phosphate flame retardant solution on their surface, and the amount of the flame retardant added is 20% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use atmospheric jet discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 8kW, and the treatment atmosphere is nitrogen; add melamine urea-formaldehyde resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 20% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot-pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0029] The performance test of Example 5 shows that the limiting oxygen index of the flame retardant particle board is 40.3%, and the static bending strength is 15.2 MPa. The limiting oxygen index of the flame retardant fiberboard is 38.8%, and the static bending strength is 25.8 MPa.
[0030] Example 6: Weigh wood particles such as wood chips and fibers, spray ammonium polyphosphate flame retardant solution on their surface, and the amount of flame retardant added is 5% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use radio frequency discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 50W, 20Hz, and the treatment atmosphere is argon; add phenolic resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 5% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0031] Example 6 Performance tests show that the limiting oxygen index of the flame retardant particle board is 32.7%, and the static bending strength is 12.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 32.1%, and the static bending strength is 26.8 MPa.
[0032] Example 7: Weigh wood particles such as wood chips and fibers, spray a guanyl urea phosphate flame retardant solution on their surface, and the amount of flame retardant added is 20% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use radio frequency discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 60W, 20Hz, and the treatment atmosphere is oxygen; add phenolic resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 20% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0033] The performance test of Example 7 shows that the limiting oxygen index of the particleboard is 43.3%, and the static bending strength is 14.8 MPa. The limiting oxygen index of the flame retardant fiberboard is 39.8%, and the static bending strength is 28.8 MPa.
[0034] Example 8: Weigh wood particles such as wood chips and fibers, spray a hydroxyethylene diphosphonic acid flame retardant solution on the surface, and the amount of the flame retardant added is 5% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, and then use microwave discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 300W, 2.45GHz, and the treatment atmosphere is oxygen; add isocyanate resin adhesive to the wood chips / fibers by spraying, stir evenly, and the amount of glue applied is 5% of the mass of the wood chips / fiber materials. The wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0035] Embodiment 8 Performance test shows that the limiting oxygen index of the flame retardant particle board is 34.9%, and the static bending strength is 10.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 32.8%, and the static bending strength is 24.0 MPa.
[0036] Example 9: Weigh wood particles such as wood chips and fibers, spray the surface with potassium salt of hexadecyl phosphate and bis(4-hydroxyphenyl)phenylphosphine oxide flame retardant solution, the amount of flame retardant added is 20% of the mass of the absolute dry wood chips. Then dry it until the moisture content is stable at 4%, then use microwave discharge plasma to treat the surface of the wood chips / fibers, the treatment power is 600W, 2.45GHz, and the treatment atmosphere is oxygen; add isocyanate resin adhesive to the wood chips / fibers by spraying, stir evenly, the amount of glue applied is 20% of the mass of the wood chips / fiber materials, and the wood chips / fibers after glue application are paved, pre-pressed, hot pressed, trimmed, sanded, etc. to obtain flame-retardant wood chips / fiberboards.
[0037] The performance test of Example 9 shows that the limiting oxygen index of the flame retardant particle board is 41.3%, and the static bending strength is 12.5 MPa. The limiting oxygen index of the flame retardant fiberboard is 39.8%, and the static bending strength is 25.8 MPa.
[0038] The invention has the beneficial effects that plasma treatment significantly enhances the flame retardant effect of various flame retardants on wood particle materials, and has a positive effect on the mechanical strength of particleboard. The particleboard prepared by the method has a limiting hydrogen index (LOI) of up to 33%-45%, and a static bending strength of up to 10.5MPa-15.7MPa, which meets the standard static bending strength (11MPa) required for load-bearing particleboard in a dry state specified in GBT 4897-2015 "Particleboard". The fiberboard prepared by the method has a limiting hydrogen index (LOI) of up to 32%-40%, and a static bending strength of up to 23MPa-29MPa, which meets the standard static bending strength (24MPa) required for load-bearing particleboard in a dry state specified in GB / T 11718-2009 "Medium Fiberboard and Density Fiberboard". The addition amount of flame retardant is 5-20%, and high-efficiency flame retardancy is achieved. In addition, the method can quickly adapt to the production process and process of existing artificial boards, and has good market promotion value.
[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the appended claims and their equivalents.
Claims
1. A method for preparing a flame retardant particle board, characterized in that: The following steps are involved: S1. Weigh wood particles such as wood shavings and fibers, spray the surface with a flame retardant solution, and then dry the particles to a moisture content of 2 to 5%. The amount of the flame retardant added is 5 to 20% of the mass of the absolutely dry wood particles. S2, performing plasma treatment on the wood particulate material after step S1; S3. Add adhesive and flame retardant to the wood particle material after plasma treatment by spraying, stir evenly, and apply adhesive in an amount of 5-20% of the mass of the absolutely dry wood particle material. Perform paving, pre-pressing, hot pressing, trimming, sanding and other treatments to obtain flame-retardant particle artificial board.
2. The method for preparing a flame retardant particle board according to claim 1, characterized in that: In the step S2, the plasma discharge mode selected is one of dielectric barrier discharge, radio frequency discharge, atmospheric jet discharge, and microwave discharge; the discharge power is 0.1-6 kW; the discharge atmosphere is one or more of nitrogen, oxygen, air, and argon, and the processing time is 3-20 s.
3. The method for preparing a flame retardant particle board according to claim 1, characterized in that: In step S1, the adhesive is selected from urea-formaldehyde resin, melamine resin, phenol-formaldehyde resin, and isocyanate adhesive.
4. The method for preparing a flame retardant particle board according to claim 1, characterized in that: The flame retardant in step S1 includes the following components: a solution of one or more of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, boric acid, borax, phytic acid, diammonium phosphate, ammonium polyphosphate, guanyl phosphate urea, hydroxyethylidene diphosphonic acid, potassium salt of hexadecanol phosphate, and bis(4-hydroxyphenyl)phenylphosphine oxide.
5. The method for preparing a flame retardant particle board according to claim 1, characterized in that: The wood particle material in step S1 is derived from one or more of wood, bamboo, and crop straw.
Citation Information
Cited By
Preparation method of green ecological composite wood floor
CN120326738A
Laminated ceiba flame-retardant composite material and preparation method thereof
CN121424502A