High-temperature-resistant stainless steel seamless tube and manufacturing method thereof

The surface treatment agent used in combination with nano ZrO2 and ZrO2-hollow microspheres form a dense thermal insulation layer, which solves the problem of the reduction of yield strength of stainless steel seamless pipes in high temperature environments, and significantly improves high temperature resistance and thermal insulation efficiency.

CN118995042AInactive Publication Date: 2024-11-22ZHEJIANG YONGSHANG SPECIAL MATERIAL CO LTD

Patent Information

Application Number
CN202411487573.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The yield strength of existing stainless steel seamless pipes is reduced in high temperature environments, and the thermal insulation capacity of existing thermal insulation coatings needs to be improved.

Method used

The surface treatment agent used in combination with nano ZrO2 and ZrO2-hollow microspheres is prepared by stirring, ball milling, high-speed centrifugal spray drying and plasma densification treatment to form a dense thermal insulation layer to improve high temperature resistance.

Benefits of technology

It significantly improves the high temperature resistance of stainless steel seamless pipes, reduces thermal conductivity, enhances thermal insulation efficiency, and has a loss rate of less than 20.9%, proving the excellent high temperature resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995042A_ABST
    Figure CN118995042A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant stainless steel seamless tube and a manufacturing method thereof, and belongs to the technical field of stainless steel tubular products, the manufacturing method comprises the following steps: S1, preparing a stainless steel seamless tube body; s2, preparing a surface treating agent; the coating is prepared from the following components in parts by weight: 22 to 30 parts of polydimethylsiloxane, 6 to 8 parts of epoxy resin, 4 to 6 parts of nano ZrO2, 5 to 7 parts of ZrO2-hollow microspheres, 9 to 11 parts of gamma-glycidoxypropyltrimethoxysilane, 0.3 to 0.5 part of a coalescing agent and 40 to 50 parts of a solvent, s3, preparing a high-temperature-resistant stainless steel seamless tube; and coating the surface treating agent on the surface of the stainless steel seamless tube body, drying, and then porcelainizing at 800-850 DEG C for 15-20 minutes to obtain the stainless steel seamless tube. The high temperature resistance of the prepared stainless steel seamless tube is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel pipes, and in particular relates to a high-temperature resistant stainless steel seamless pipe and a manufacturing method thereof. Background Art

[0002] Stainless steel seamless pipe is a long steel strip with a hollow cross-section and no seams around it. Common stainless steel seamless pipe materials include 304, 316L, 321, etc. These materials have different corrosion resistance and mechanical properties. Stainless steel seamless pipes have various specifications, ranging from 54mm to 480mm in diameter and 0.5mm to 45mm in wall thickness. It has excellent performance and a wide range of applications. It can be used in pipeline systems for conveying corrosive media in the petroleum and chemical industries, in the medical and food industries for the manufacture of medical devices and food processing equipment, in the light industry and mechanical instrumentation industries for various mechanical structural components, and in the construction industry for water supply pipeline systems. Stainless steel seamless pipes have good corrosion resistance, especially for chemical media such as acids, alkalis, and salts. In addition, it also has a high yield strength, which is suitable for high-pressure and high-strength applications.

[0003] Since high temperature will cause the atomic vibration in the metal lattice to intensify, thereby weakening the bonding force between atoms, the yield strength of stainless steel materials will decrease with the increase of temperature. Therefore, in order to improve the high temperature resistance of seamless pipes made of stainless steel materials, in the prior art, a treatment agent is coated on the surface of the seamless pipe to form a thermal insulation coating to achieve a thermal insulation effect. Inorganic particles are used in the thermal insulation coating to achieve a thermal insulation effect. For example, nano zirconium dioxide, with its high melting point, high resistivity and low thermal expansion coefficient, has become an effective inorganic thermal insulation particle and is widely used in various high temperature and thermal insulation occasions. But at the same time, zirconium dioxide, as an inorganic thermal insulation particle, is used in the coating, and its thermal insulation ability needs to be further improved. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a high temperature resistant stainless steel seamless pipe and a manufacturing method thereof, which significantly improves the high temperature resistance of the manufactured stainless steel seamless pipe.

[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for manufacturing a high temperature resistant stainless steel seamless pipe, comprising the following steps: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.032-0.035%, Cr: 18-20%, Ni: 19-22%, Si: 0.6-0.8%, Mn: 0.4-0.5%, Mo: 0.6-0.8%, Ce: 0.08-0.1%, Al: 0.02-0.03%, S≤0.003%, P≤0.002%, and the balance is iron and unavoidable impurities; S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 22-30 parts of polydimethylsiloxane, 6-8 parts of epoxy resin, 4-6 parts of nano ZrO2, 5-7 parts of ZrO2-hollow microspheres, 9-11 parts of γ-glycidyloxypropyltrimethoxysilane, 0.3-0.5 parts of film-forming aid and 40-50 parts of solvent; S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained in S2 is coated on the surface of the stainless steel seamless pipe body obtained in S1, dried, and then vitrified at 800-850°C for 15-20 minutes to obtain a high temperature resistant stainless steel seamless pipe.

[0006] Furthermore, the specific operating steps of S2 are as follows: mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres to obtain component a; mix γ-glycidyloxypropyltrimethoxysilane, film-forming aid and solvent to obtain component b; mix component a and component b to obtain a surface treatment agent.

[0007] Furthermore, the film-forming aid is propylene glycol methyl ether acetate; and the solvent includes acetone and / or ethyl acetate.

[0008] Furthermore, the preparation method of the ZrO2-hollow microspheres is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of (9-10):10 to obtain a mixture, add 0.4-0.6% of the mass of the mixture dispersant, mix well, and obtain a mixture; A2, put the mixture obtained in A1 into a vertical ball mill, add ball milling medium, ball mill at 900-1000r / min for 1-1.2h, add binder, and continue ball milling at the same speed for 10min to obtain ball mill material; A3, put the ball mill obtained in A2 into a mixer, stir at 180-200 r / min for 30-40 min, add 0.1% of the mass of the mixture defoamer every 10 min to obtain a defoaming material; A4, granulating the defoaming material obtained in A3 using a high-speed centrifugal spray dryer, and then drying and sieving to obtain agglomerated powder with a particle size of 45-60 μm; A5, heating the agglomerated powder obtained in A4 to 890-900°C in a resistance furnace at a heating rate of 5°C / min, keeping the temperature for 1-1.1h, and then cooling to room temperature with the furnace to obtain calcined powder; A6. The calcined powder obtained in A5 is subjected to plasma densification treatment to obtain ZrO2-hollow microspheres.

[0009] Furthermore, in A1, the dispersant is n-octanol.

[0010] Furthermore, in A2, the binder is polyvinyl alcohol; the mass of the binder is 0.1-0.12% of the mass of the mixture.

[0011] Furthermore, in A3, the defoaming agent is a GPE type polyether defoaming agent.

[0012] Furthermore, in A4, the inlet temperature of the high-speed centrifugal spray dryer is 250-260°C, the outlet temperature is 140-160°C, and the atomizing disk rotation speed is 10000r / min.

[0013] Furthermore, the specific operation of A6 is: the calcined powder obtained by A5 is fed into the plasma spraying equipment through a feeding device, and the parameters are current 400A, voltage 40V, main gas argon flow rate 1300l / h and powder feeding rate 13L / min; the calcined powder is instantly heated in the argon plasma flame flow with 14700K, and is rapidly cooled after being injected into pure water, and its grains will not grow larger, and then dried to obtain ZrO2-hollow microspheres.

[0014] In a second aspect, the present invention provides a high temperature resistant stainless steel seamless pipe, which is produced by the above-mentioned manufacturing method.

[0015] This application has the following beneficial effects: 1. In the surface treatment agent of the present invention, nano ZrO2 and ZrO2-hollow microspheres are used in combination, and both have good high-temperature stability and chemical inertness, and can maintain their structure and performance unchanged under high-temperature environment; the internal cavity of ZrO2-hollow microspheres can also effectively block the heat transfer path, effectively reduce thermal conductivity, and thus enhance thermal insulation performance; ZrO2-hollow microspheres also have good dispersibility and can be evenly dispersed in the coating, but at the same time, the particle size of ZrO2-hollow microspheres made of nano ZrO2 is greatly increased, which will lead to an increase in the number of voids in the coating, and nano ZrO2 can just fill the voids between ZrO2-hollow microspheres in the coating well, forming a denser thermal insulation layer, reducing the channels for heat penetration, thereby improving the thermal insulation efficiency and enhancing the high temperature resistance of the obtained product.

[0016] 2. In the preparation of ZrO2-hollow microspheres of the present invention, heat treatment is performed in a resistance furnace to burn off the organic binder, while allowing the small nanoparticles in a single large particle aggregate to have a weak connection, while there is no connection between the large particles, thereby ensuring that the nanoparticles do not grow while ensuring that the powder has a high density and low porosity; and plasma densification treatment, instantaneous high-temperature heating and rapid cooling are performed, so that the nanoparticles on the surface of the calcined powder are melted together after the melting and solidification process to form a smooth micron-level thin-walled shell, thereby forming a hollow micropowder with a micro-nano hollow structure. Since the surface of the hollow micropowder is very smooth and the density is greatly improved, its fluidity and loose density are greatly improved, and the overall thermal insulation performance is improved, which is more conducive to improving the high temperature resistance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 , a comparative trend chart of yield strength test data of products obtained in Examples 1-6 of the present invention and Comparative Examples 1-6 at room temperature and 500°C; Figure 2 , a comparative trend chart of the loss rate of the yield strength test data of the products obtained in Examples 1-6 of the present invention and Comparative Examples 1-6 at 500°C compared with the yield strength test data at room temperature. DETAILED DESCRIPTION

[0018] The present application is further described in detail below in conjunction with embodiments.

[0019] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0020] Example 1: (1) Preparation of ZrO2-hollow microspheres, the preparation method is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9.5:10 to obtain a mixture, add 0.5% of the mass of the mixture as a dispersant n-octanol, mix well, and obtain a mixture. Among them, nano ZrO2 (content ≥99.9%, specification VK-R30D) was purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd. n-octanol (superior grade, content ≥99.9%) was purchased from Jinan Mingyang Chemical Co., Ltd.

[0021] A2. Put the mixture obtained in A1 into a vertical ball mill, add 5mm ball milling media, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 950r / min for 1.1h, add the binder polyvinyl alcohol, the mass of which is 0.11% of the mass of the mixture, and continue ball milling at the same speed for 10min to obtain ball milling material. Among them, polyvinyl alcohol, brand PVA100-27 (1799D), degree of polymerization 1750±50, was purchased from Sinopec Shanghai Petrochemical Co., Ltd.

[0022] A3, the ball mill obtained in A2 was put into a mixer, stirred at 190r / min for 35min, during which 0.1% of the mass of the mixture was added to the GPE type polyether defoamer every 10min to obtain a defoaming material. Among them, the GPE-3000 polyether defoamer was purchased from Hai'an Petrochemical Plant in Jiangsu Province. The main function of the defoamer is to eliminate bubbles in the mixture to prevent product defects caused by the presence of bubbles during the subsequent spray drying and calcination process.

[0023] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 255°C, an outlet temperature of 148°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0024] A5. Heat the agglomerated powder obtained in A4 to 895°C in a resistance furnace at a heating rate of 5°C / min, keep it at that temperature for 1 hour, and then cool it to room temperature in the furnace to obtain a calcined powder.

[0025] A6. The calcined powder obtained by A5 is subjected to plasma densification treatment. Specifically, the calcined powder obtained by A5 is fed into a plasma spraying device with parameters of current 400A, voltage 40V, argon flow rate 1300l / h and powder feeding rate 13L / min. The calcined powder is instantly heated in an argon plasma flame flow with a temperature of 14700K, and is rapidly cooled after being injected into pure water, so that the grains thereof will not grow significantly. The powder is then dried to obtain ZrO2-hollow microspheres.

[0026] (2) Manufacturing a high temperature resistant stainless steel seamless pipe, the manufacturing method comprising the following steps: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.033%, Cr: 19.2%, Ni: 20.5%, Si: 0.7%, Mn: 0.45%, Mo: 0.7%, Ce: 0.09%, Al: 0.025%, S: 0.002%, P: 0.0015%, and the remainder is iron and unavoidable impurities.

[0027] The preparation process is an existing technology. Specifically, after continuous casting to obtain a tube billet, it is heated at 1260°C for 50 minutes in a ring heating furnace, and then piercing (1240°C) and tube rolling (outlet temperature 1080°C) operations are performed, and then finish rolling (outlet temperature 950°C) and straightening treatment are performed to obtain a tube. Then, water is sprayed to accelerate cooling to 450°C at a cooling rate of about 25°C / s, and then air-cooled to room temperature to obtain a stainless steel seamless tube body.

[0028] S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 26 parts of polydimethylsiloxane, 7 parts of epoxy resin, 5 parts of nano ZrO2, 6 parts of ZrO2-hollow microspheres, 10 parts of γ-glycidyloxypropyltrimethoxysilane, 0.4 parts of film-forming aid and 45 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres, stir at 180r / min for 20 minutes in a disperser to obtain component a. Mix γ-glycidyloxypropyl trimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30 minutes in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50 minutes in a disperser to obtain a surface treatment agent.

[0029] Among them, the film-forming aid is propylene glycol methyl ether acetate (superior grade), purchased from Dongguan United Chemical Group Co., Ltd. The solvent is acetone. Polydimethylsiloxane was purchased from Nanjing Danpei Chemical Co., Ltd. The epoxy resin is bisphenol F type resin 170, purchased from Shanghai Kaiyin Chemical Co., Ltd. γ-glycidyl ether oxypropyl trimethoxy silane (KH-560) was purchased from Shandong Yousuo Chemical Technology Co., Ltd.

[0030] S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained from S2 is coated on the surface of the stainless steel seamless pipe body obtained from S1, dried, and then vitrified at 840°C for 18 minutes to form a coating with a thickness of 63.5 μm, thereby obtaining a high temperature resistant stainless steel seamless pipe.

[0031] Example 2: The difference between this example and Example 1 is that: (1) ZrO2-hollow microspheres are prepared by the following method: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9:10 to obtain a mixture, add 0.4% by mass of the mixture of dispersant n-octanol, mix well, and obtain a mixture.

[0032] A2. Put the mixture obtained in A1 into a vertical ball mill, add Ø5mm ball milling media, the ball-to-material mass ratio is 5:1, and after ball milling at 900r / min for 1h, add binder polyvinyl alcohol, the mass of polyvinyl alcohol is 0.1% of the mass of the mixture, and continue ball milling at the same speed for 10min to obtain ball mill material.

[0033] A3. The ball mill obtained in A2 was put into a mixer and stirred at 180 r / min for 30 min. During the stirring, 0.1% of the mass of the mixture was added with a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0034] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 250°C, an outlet temperature of 140°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0035] A5. Heat the agglomerated powder obtained in A4 to 890°C in a resistance furnace at a heating rate of 5°C / min, keep it at that temperature for 1 hour, and then cool it to room temperature in the furnace to obtain a calcined powder.

[0036] A6. The calcined powder obtained by A5 is subjected to plasma densification treatment. Specifically, the calcined powder obtained by A5 is fed into a plasma spraying device with parameters of current 400A, voltage 40V, argon flow rate 1300l / h and powder feeding rate 13L / min. The calcined powder is instantly heated in an argon plasma flame flow with a temperature of 14700K, and is rapidly cooled after being injected into pure water, so that the grains thereof will not grow significantly. The powder is then dried to obtain ZrO2-hollow microspheres.

[0037] Example 3: The difference between this example and Example 1 is that: (1) ZrO2-hollow microspheres are prepared by the following method: A1. Mix nano ZrO2 and deionized water in a mass ratio of 1:1 to obtain a mixture, add 0.6% of the mass of the mixture as a dispersant n-octanol, mix well, and obtain a mixture.

[0038] A2. Put the mixture obtained in A1 into a vertical ball mill, add Ø5mm ball milling media, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 1000r / min for 1.2h, add the binder polyvinyl alcohol, the mass of which is 0.12% of the mass of the mixture, and continue ball milling at the same speed for 10min to obtain ball mill material.

[0039] A3. The ball mill obtained in A2 was put into a mixer and stirred at 200 r / min for 40 min. During this period, 0.1% of the mass of the mixture was added to a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0040] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 260°C, an outlet temperature of 154°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0041] A5. The agglomerated powder obtained in A4 was heated to 900°C in a resistance furnace at a heating rate of 5°C / min, kept at this temperature for 1.1 h, and then cooled to room temperature in the furnace to obtain a calcined powder.

[0042] A6. The calcined powder obtained by A5 is subjected to plasma densification treatment. Specifically, the calcined powder obtained by A5 is fed into a plasma spraying device with parameters of current 400A, voltage 40V, argon flow rate 1300l / h and powder feeding rate 13L / min. The calcined powder is instantly heated in an argon plasma flame flow with a temperature of 14700K, and is rapidly cooled after being injected into pure water, so that the grains thereof will not grow significantly. The powder is then dried to obtain ZrO2-hollow microspheres.

[0043] Embodiment 4: The difference between this embodiment and embodiment 1 is that: (2) manufacturing a high temperature resistant stainless steel seamless pipe, the manufacturing method thereof comprises the following steps: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.032%, Cr: 18%, Ni: 19%, Si: 0.6%, Mn: 0.4%, Mo: 0.6%, Ce: 0.08%, Al: 0.02%, S: 0.002%, P: 0.0013%, and the remainder is iron and unavoidable impurities.

[0044] S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 22 parts of polydimethylsiloxane, 6 parts of epoxy resin, 4 parts of nano ZrO2, 5 parts of ZrO2-hollow microspheres, 9 parts of γ-glycidyloxypropyltrimethoxysilane, 0.3 parts of film-forming aid and 40 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres, stir at 180r / min for 20 minutes in a disperser to obtain component a. Mix γ-glycidyloxypropyl trimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30 minutes in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50 minutes in a disperser to obtain a surface treatment agent.

[0045] S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained in S2 is coated on the surface of the stainless steel seamless pipe body obtained in S1, dried, and then vitrified at 800°C for 15 minutes to form a coating with a thickness of 64.2 μm, thereby obtaining a high temperature resistant stainless steel seamless pipe.

[0046] Embodiment 5: The difference between this embodiment and embodiment 1 is that: (2) manufacturing a high temperature resistant stainless steel seamless pipe, the manufacturing method thereof comprises the following steps: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.035%, Cr: 20%, Ni: 22%, Si: 0.8%, Mn: 0.5%, Mo: 0.8%, Ce: 0.1%, Al: 0.03%, S: 0.0024%, P: 0.0016%, and the remainder is iron and unavoidable impurities.

[0047] S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 30 parts of polydimethylsiloxane, 8 parts of epoxy resin, 6 parts of nano ZrO2, 7 parts of ZrO2-hollow microspheres, 11 parts of γ-glycidyloxypropyltrimethoxysilane, 0.5 parts of film-forming aid and 50 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres, stir at 180r / min for 20 minutes in a disperser to obtain component a. Mix γ-glycidyloxypropyl trimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30 minutes in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50 minutes in a disperser to obtain a surface treatment agent.

[0048] S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained from S2 is coated on the surface of the stainless steel seamless pipe body obtained from S1, dried, and then vitrified at 850°C for 20 minutes to form a coating with a thickness of 63.3 μm, thereby obtaining a high-temperature resistant stainless steel seamless pipe.

[0049] Embodiment 6: The difference between this embodiment and embodiment 1 is that: (2) manufacturing a high temperature resistant stainless steel seamless pipe, the manufacturing method thereof comprises the following steps: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.034%, Cr: 18.8%, Ni: 21.5%, Si: 0.68%, Mn: 0.47%, Mo: 0.72%, Ce: 0.088%, Al: 0.022%, S: 0.0025%, P: 0.0015%, and the balance is iron and unavoidable impurities.

[0050] S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 24 parts of polydimethylsiloxane, 7.4 parts of epoxy resin, 5.2 parts of nano ZrO2, 6.8 parts of ZrO2-hollow microspheres, 10.5 parts of γ-glycidyloxypropyltrimethoxysilane, 0.44 parts of film-forming aid and 48 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres, stir at 180r / min for 20 minutes in a disperser to obtain component a. Mix γ-glycidyloxypropyl trimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30 minutes in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50 minutes in a disperser to obtain a surface treatment agent.

[0051] S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained from S2 is coated on the surface of the stainless steel seamless pipe body obtained from S1, dried, and then vitrified at 840°C for 19 minutes to form a coating with a thickness of 62.3 μm, thereby obtaining a high-temperature resistant stainless steel seamless pipe.

[0052] Comparative Example 1: The difference between this comparative example and Example 1 is that in the preparation of the surface treatment agent, ZrO2-hollow microspheres are replaced by nano ZrO2; that is, only nano ZrO2 is used.

[0053] Specifically, S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 26 parts of polydimethylsiloxane, 7 parts of epoxy resin, 11 parts of nano ZrO2, 10 parts of γ-glycidyloxypropyltrimethoxysilane, 0.4 parts of film-forming aid and 45 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin and nano ZrO2, stir at 180r / min for 20min in a disperser to obtain component a. Mix γ-glycidyloxypropyl trimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30min in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50min in a disperser to obtain a surface treatment agent.

[0054] Comparative Example 2: The difference between this comparative example and Example 1 is that in the preparation of the surface treatment agent, nano ZrO2 is replaced by ZrO2-hollow microspheres; that is, only ZrO2-hollow microspheres are used.

[0055] Specifically, S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 26 parts of polydimethylsiloxane, 7 parts of epoxy resin, 11 parts of ZrO2-hollow microspheres, 10 parts of γ-glycidyloxypropyltrimethoxysilane, 0.4 parts of film-forming aid and 45 parts of solvent; The specific operation steps are as follows: Mix polydimethylsiloxane, epoxy resin and ZrO2-hollow microspheres, stir at 180r / min for 20 minutes in a disperser to obtain component a. Mix γ-glycidyloxypropyltrimethoxysilane, film-forming aid and solvent, stir at 150r / min for 30 minutes in a disperser to obtain component b. Mix component a and component b, stir at 200r / min for 50 minutes in a disperser to obtain a surface treatment agent.

[0056] Comparative Example 3: The difference between this comparative example and Example 1 is that in the preparation of ZrO2-hollow microspheres, step A5 is heated to 700°C.

[0057] Specifically, ZrO2-hollow microspheres are prepared, and the preparation method thereof is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9.5:10 to obtain a mixture, add 0.5% by mass of the mixture of dispersant n-octanol, mix well, and obtain a mixture.

[0058] A2. Put the mixed material obtained in A1 into a vertical ball mill, add Ø5mm ball milling medium, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 950 r / min for 1.1 h, add the binder polyvinyl alcohol, the mass of which is 0.11% of the mass of the mixture, and continue ball milling at the same speed for 10 min to obtain ball mill material.

[0059] A3. The ball mill obtained in A2 was put into a mixer and stirred at 190 r / min for 35 min. During the stirring, 0.1% of the mass of the mixture was added with a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0060] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 255°C, an outlet temperature of 148°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0061] A5. Heat the agglomerated powder obtained in A4 to 700°C in a resistance furnace at a heating rate of 5°C / min, keep it at that temperature for 1 hour, and then cool it to room temperature in the furnace to obtain a calcined powder.

[0062] A6. The calcined powder obtained by A5 is subjected to plasma densification treatment. Specifically, the calcined powder obtained by A5 is fed into a plasma spraying device with parameters of current 400A, voltage 40V, argon flow rate 1300l / h and powder feeding rate 13L / min. The calcined powder is instantly heated in an argon plasma flame flow with a temperature of 14700K, and is rapidly cooled after being injected into pure water, so that the grains thereof will not grow significantly. The powder is then dried to obtain ZrO2-hollow microspheres.

[0063] Comparative Example 4: The difference between this comparative example and Example 1 is that in the preparation of ZrO2-hollow microspheres, step A5 is heated to 1100°C.

[0064] Specifically, ZrO2-hollow microspheres are prepared, and the preparation method thereof is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9.5:10 to obtain a mixture, add 0.5% by mass of the mixture of dispersant n-octanol, mix well, and obtain a mixture.

[0065] A2. Put the mixed material obtained in A1 into a vertical ball mill, add Ø5mm ball milling medium, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 950 r / min for 1.1 h, add the binder polyvinyl alcohol, the mass of which is 0.11% of the mass of the mixture, and continue ball milling at the same speed for 10 min to obtain ball mill material.

[0066] A3. The ball mill obtained in A2 was put into a mixer and stirred at 190 r / min for 35 min. During the stirring, 0.1% of the mass of the mixture was added with a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0067] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 255°C, an outlet temperature of 148°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0068] A5. Heat the agglomerated powder obtained in A4 to 1100°C in a resistance furnace at a heating rate of 5°C / min, keep it at that temperature for 1 hour, and then cool it to room temperature in the furnace to obtain a calcined powder.

[0069] A6. The calcined powder obtained by A5 is subjected to plasma densification treatment. Specifically, the calcined powder obtained by A5 is fed into a plasma spraying device with parameters of current 400A, voltage 40V, argon flow rate 1300l / h and powder feeding rate 13L / min. The calcined powder is instantly heated in an argon plasma flame flow with a temperature of 14700K, and is rapidly cooled after being injected into pure water, so that the grains thereof will not grow significantly. The powder is then dried to obtain ZrO2-hollow microspheres.

[0070] Comparative Example 5: The difference between this comparative example and Example 1 is that in the preparation of ZrO2-hollow microspheres, step A6 is deleted.

[0071] Specifically, ZrO2-hollow microspheres are prepared, and the preparation method thereof is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9.5:10 to obtain a mixture, add 0.5% by mass of the mixture of dispersant n-octanol, mix well, and obtain a mixture.

[0072] A2. Put the mixed material obtained in A1 into a vertical ball mill, add Ø5mm ball milling medium, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 950 r / min for 1.1 h, add the binder polyvinyl alcohol, the mass of which is 0.11% of the mass of the mixture, and continue ball milling at the same speed for 10 min to obtain ball mill material.

[0073] A3. The ball mill obtained in A2 was put into a mixer and stirred at 190 r / min for 35 min. During the stirring, 0.1% of the mass of the mixture was added with a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0074] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 255°C, an outlet temperature of 148°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0075] A5. The agglomerated powder obtained in A4 was heated to 895°C in a resistance furnace at a heating rate of 5°C / min, kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a calcined powder, which was used as ZrO2-hollow microspheres.

[0076] Comparative Example 6: The difference between this comparative example and Example 1 is that in the preparation of ZrO2-hollow microspheres, step A5 is heated to 700°C, and step A6 is deleted.

[0077] Specifically, ZrO2-hollow microspheres are prepared, and the preparation method thereof is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of 9.5:10 to obtain a mixture, add 0.5% by mass of the mixture of dispersant n-octanol, mix well, and obtain a mixture.

[0078] A2. Put the mixed material obtained in A1 into a vertical ball mill, add Ø5mm ball milling medium, the ball-to-material mass ratio is 5:1, and after ball milling at a speed of 950 r / min for 1.1 h, add the binder polyvinyl alcohol, the mass of which is 0.11% of the mass of the mixture, and continue ball milling at the same speed for 10 min to obtain ball mill material.

[0079] A3. The ball mill obtained in A2 was put into a mixer and stirred at 190 r / min for 35 min. During the stirring, 0.1% of the mass of the mixture was added with a GPE type polyether defoamer every 10 min to obtain a defoaming material.

[0080] A4. Granulate the defoaming material obtained in A3 using a high-speed centrifugal spray dryer with an inlet temperature of 255°C, an outlet temperature of 148°C, and an atomizing disk speed of 10,000 r / min. Then put it in an oven with a drying temperature of 105°C and a drying time of 1 hour to remove residual moisture. Then screen out agglomerated powder with a particle size of 45-60 μm.

[0081] A5. The agglomerated powder obtained in A4 was heated to 700°C in a resistance furnace at a heating rate of 5°C / min, kept at this temperature for 1 hour, and then cooled to room temperature in the furnace to obtain a calcined powder, which was used as ZrO2-hollow microspheres.

[0082] Test example: Test method: According to the contents specified in Examples 1-6 and Comparative Examples 1-12, (cut) a 50mm×25mm×3mm stainless steel seamless pipe steel sample; at room temperature 25°C and 500°C, the yield strength of the steel sample was tested with a tensile testing machine, with a tensile speed of 15mm / min; and the loss rate was calculated, loss rate = (yield strength at room temperature - yield strength at 500°C) / yield strength at room temperature * 100%; the smaller the loss rate, the stronger the high temperature resistance.

[0083] Test results: See Table 1.

[0084] Table 1. Test example data Yield strength at room temperature / MPa Yield strength at 500℃ / MPa Loss rate / % Example 1 887.5 705.9 20.5 Example 2 891.3 705.3 20.9 Example 3 885.4 708.1 20.0 Example 4 883.7 699.5 20.8 Example 5 892.2 706.8 20.8 Example 6 889.3 710.6 20.1 Comparative Example 1 891.2 608.8 31.7 Comparative Example 2 885.7 582.3 34.3 Comparative Example 3 881.4 666.2 24.4 Comparative Example 4 883.4 674.5 23.6 Comparative Example 5 888.2 635.7 28.4 Comparative Example 6 879.9 618.1 29.8 Result analysis: Analyze examples 1-6 and combine the data in Table 1 and Figure 1-Figure 2 It can be seen that the yield strength measured at 500°C has a loss rate as low as 20.9% compared with the yield strength measured at room temperature, indicating that the product prepared by the present invention has excellent high temperature resistance.

[0085] Analyze Comparative Example 1 and Comparative Example 2 and combine the data in Table 1 and Figure 1-Figure 2 It can be seen that the loss rate measured in Comparative Example 2 is 34.3%, which is significantly greater than the loss rate of 31.7% measured in Comparative Example 1, indicating that in the preparation of the surface treatment agent, directly replacing the nano ZrO2 with the ZrO2-hollow microspheres of the present invention for use, the loss rate of the obtained product does not decrease but increases, that is, the high temperature resistance of the obtained product does not increase but decreases. This shows that using the nano ZrO2 made into the ZrO2-hollow microspheres of the present invention for use has a negative effect on the high temperature resistance of the product.

[0086] This is because nano ZrO2 is made into ZrO2-hollow microspheres. Although the ordered hollow structure effectively blocks the heat transfer path through its internal cavity, reduces heat transfer, and can enhance the thermal insulation performance; but at the same time, the increase in particle size will also lead to more voids / pores in the coating. These randomly distributed voids will cause heat to be more easily transferred through convection and radiation, becoming a potential channel for heat transfer, resulting in the weakening of the overall thermal insulation effect of the coating.

[0087] Analyze Example 1 and Comparative Example 1 and combine the data in Table 1 and Figure 1-Figure 2 It can be seen that the loss rate measured in Example 1 is 20.5%, which is significantly lower than the loss rate of 31.7% measured in Comparative Example 1, indicating that in the preparation of the surface treatment agent, part of the nano ZrO2 is replaced by the ZrO2-hollow microspheres of the present invention according to the proportion of the present invention, and the loss rate of the obtained product is significantly reduced, that is, the high temperature resistance of the obtained product is significantly improved.

[0088] Analyze Example 1 and Comparative Examples 3-6 and combine the data in Table 1 and Figure 1-Figure 2 It can be seen that the loss rate measured in Comparative Example 3 is 24.4%, which is significantly greater than the loss rate of 20.5% measured in Example 1, indicating that in the preparation of ZrO2-hollow microspheres, the heating temperature in step A5 is too low (as low as 700°C), which will lead to an increase in the loss rate of the obtained product, that is, the high temperature resistance of the obtained product is reduced. The loss rate measured in Comparative Example 4 is 23.6%, which is significantly greater than the loss rate of 20.5% measured in Example 1, indicating that in the preparation of ZrO2-hollow microspheres, the heating temperature in step A5 is too high (as high as 1100°C), which will also lead to an increase in the loss rate of the obtained product, that is, the high temperature resistance of the obtained product is reduced.

[0089] This is because, if the temperature is too low, the small nanoparticles cannot be connected together, and the large agglomerate particles cannot be well densified; while if the temperature is too high, the large agglomerate particles will be connected together, and the nanocrystals will grow rapidly, affecting the fluidity. Only by following the reasonable heat treatment temperature defined in the present invention can the purpose of burning off the organic binder be achieved and the relevant properties of the nanoagglomerate powder be improved.

[0090] The loss rate measured in Comparative Example 5 was 28.4%, which was significantly higher than the loss rate of 20.5% measured in Example 1, indicating that in the preparation of ZrO2-hollow microspheres, deleting step A5, i.e. not performing plasma densification treatment, would lead to an increase in the loss rate of the obtained product, i.e., a decrease in the high temperature resistance of the obtained product.

[0091] The loss rate measured in Comparative Example 6 is 29.8%> the loss rate measured in Comparative Example 5 is 28.4% / the loss rate measured in Comparative Example 3 is 24.4%> the loss rate measured in Example 1 is 20.5%, indicating that in the preparation of ZrO2-hollow microspheres, there is a synergistic effect between the heating limiting temperature in step A5 and the plasma densification treatment in step A6, which can synergistically improve the high temperature resistance of the obtained product.

[0092] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0093] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for manufacturing a high temperature resistant stainless steel seamless pipe, characterized in that: The steps include: S1. Prepare a stainless steel seamless pipe body; The composition of the stainless steel seamless pipe body includes, by mass percentage, C: 0.032-0.035%, Cr: 18-20%, Ni: 19-22%, Si: 0.6-0.8%, Mn: 0.4-0.5%, Mo: 0.6-0.8%, Ce: 0.08-0.1%, Al: 0.02-0.03%, S≤0.003%, P≤0.002%, and the balance is iron and unavoidable impurities; S2, preparing a surface treatment agent; The surface treatment agent comprises, by weight, 22-30 parts of polydimethylsiloxane, 6-8 parts of epoxy resin, 4-6 parts of nano ZrO2, 5-7 parts of ZrO2-hollow microspheres, 9-11 parts of γ-glycidyloxypropyltrimethoxysilane, 0.3-0.5 parts of film-forming aid and 40-50 parts of solvent; S3, preparing high temperature resistant stainless steel seamless pipe; The surface treatment agent obtained in S2 is coated on the surface of the stainless steel seamless pipe body obtained in S1, dried, and then vitrified at 800-850°C for 15-20 minutes to obtain a high temperature resistant stainless steel seamless pipe.

2. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 1, characterized in that: The specific operating steps of S2 are as follows: mix polydimethylsiloxane, epoxy resin, nano ZrO2 and ZrO2-hollow microspheres to obtain component a; mix γ-glycidyloxypropyltrimethoxysilane, film-forming aid and solvent to obtain component b; mix component a and component b to obtain a surface treatment agent.

3. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 2, characterized in that: The film-forming aid is propylene glycol methyl ether acetate; and the solvent includes acetone and / or ethyl acetate.

4. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 1 or 2, characterized in that: The preparation method of the ZrO2-hollow microspheres is as follows: A1. Mix nano ZrO2 and deionized water in a mass ratio of (9-10):10 to obtain a mixture, add 0.4-0.6% of the mass of the mixture dispersant, mix well, and obtain a mixture; A2, put the mixture obtained in A1 into a ball mill, add ball milling medium, ball mill at 900-1000r / min for 1-1.2h, add binder, and continue ball milling for 10min to obtain ball mill material; A3, put the ball mill obtained in A2 into a mixer, stir at 180-200 r / min for 30-40 min, add 0.1% of the mass of the mixture of defoamer every 10 min to obtain a defoaming material; A4, granulating the defoaming material obtained in A3 using a high-speed centrifugal spray dryer, and then drying and sieving to obtain agglomerated powder with a particle size of 45-60 μm; A5, heating the agglomerated powder obtained in A4 to 890-900°C in a resistance furnace at a heating rate of 5°C / min, keeping the temperature for 1-1.1h, and then cooling to room temperature with the furnace to obtain calcined powder; A6. The calcined powder obtained in A5 is subjected to plasma densification treatment to obtain ZrO2-hollow microspheres.

5. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 4, characterized in that: In A1, the dispersant is n-octanol.

6. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 4, characterized in that: In A2, the binder is polyvinyl alcohol; the mass of the binder is 0.1-0.12% of the mass of the mixture.

7. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 4, characterized in that: In A3, the defoamer is a GPE type polyether defoamer.

8. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 4, characterized in that: In A4, the inlet temperature of the high-speed centrifugal spray dryer is 250-260°C, the outlet temperature is 140-160°C, and the atomizing disk speed is 10000r / min.

9. The method for manufacturing a high temperature resistant stainless steel seamless pipe according to claim 4, characterized in that: The specific operation of A6 is: the calcined powder obtained in A5 is sent to the plasma spraying equipment, the calcined powder is instantly heated in the argon plasma flame flow with 14700K, and is quickly cooled after being injected into pure water, and then dried to obtain ZrO2-hollow microspheres.

10. A high temperature resistant stainless steel seamless pipe, characterized in that: The method is prepared by the manufacturing method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Solvent type functional coating with good solar energy absorption and infrared radiation performance and preparation method of solvent type functional coating

    CN113462285A

  • High-temperature-resistant stainless steel seamless steel pipe and surface treatment process thereof

    CN113667362A

  • High-temperature-resistant stainless steel seamless steel pipe and processing method thereof

    CN113999580A

  • Refractory castable for furnace lining of roasting furnace for preparing positive electrode material of lithium battery

    CN117865698A

  • Tunnel porcelainized coating suitable for high-altitude areas and preparation method of tunnel porcelainized coating

    CN118725734A

Cited By

  • Surface strengthening method for cast steel special-shaped pipe fitting

    CN119529638A

  • High-temperature-resistant seamless steel tube and preparation process thereof

    CN119685683A