Preparation method and application of Cu-based catalyst taking CeO2 as carrier

By using CeO2 as a support and preparing Cu/CeO2 catalysts under different temperature conditions, the problems of insufficient activity, poor selectivity and insufficient stability of traditional Cu-based catalysts are solved, and efficient catalytic performance and long-term time are achieved in the field of electrocatalytic CO2 reduction Stability has promoted the recycling of carbon resources.

CN118996490APending Publication Date: 2024-11-22EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411089190.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional single Cu-based catalysts have problems such as insufficient activity, poor selectivity and insufficient stability in the field of electrocatalytic CO2 reduction, resulting in low conversion efficiency and deterioration of performance, limiting their industrial applications.

Method used

Rod-shaped CeO2 is prepared by using CeO2 as a support, and Cu(NO3)2 and CeO2 are mixed under different temperature conditions to ensure uniform loading of Cu. High-performance Cu/CeO2 catalyst is prepared by calcining to enhance the catalyst activity, selectivity and stability.

Benefits of technology

It significantly improves the catalytic activity and selectivity of the catalyst, extends the service life, improves the concentration and economic benefits of the target products, and promotes the recycling of carbon resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996490A_ABST
    Figure CN118996490A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a Cu-based catalyst with CeO2 as a carrier, and relates to the technical field of carbon dioxide catalytic conversion, the catalyst is composed of a Cu active component and a CeO2 carrier, by means of the elaborately designed preparation method, Cu is successfully and evenly loaded on the CeO2 carrier with different crystal face proportions, and the catalyst is prepared. Due to the unique structural design, the catalyst can show more excellent catalytic performance in the electrocatalytic carbon dioxide reduction process, the CO2 adsorption capacity of the catalyst is enhanced through interaction between Cu and CeO2, transfer of electrons and stability of reaction intermediates are promoted, the activity of the catalyst is remarkably improved, and the catalytic performance of the catalyst is improved. The different crystal face proportions of the CeO2 carrier provide diversified active sites for the reaction, the selectivity of the catalyst to the target product is further improved, the product distribution is more concentrated, and the purification and processing of subsequent products are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalytic conversion of carbon dioxide, and in particular to a preparation method and application of a Cu-based catalyst using CeO2 as a carrier. Background Art

[0002] With the acceleration of the global industrialization process, the excessive consumption of fossil fuels has led to a sharp increase in the concentration of carbon dioxide (CO2) in the atmosphere, causing serious environmental problems such as the intensification of the greenhouse effect and climate change, posing a severe challenge to the sustainable development of natural ecosystems and human society. Therefore, it is necessary to explore and develop efficient CO2 conversion and utilization technologies, especially through the electrocatalytic reduction of CO2, to achieve the conversion of CO2 into high value-added chemicals under normal temperature and pressure conditions. Therefore, the development of a preparation method and application of a Cu-based catalyst with CeO2 as the carrier will not only help alleviate environmental pressure, but also promote the recycling of carbon resources.

[0003] Among the numerous electrocatalytic CO2 reduction catalysts, Cu-based catalysts can catalyze the conversion of CO2 into a variety of hydrocarbon-containing compounds due to their unique properties, showing broad application prospects. However, traditional single Cu-based catalysts face many bottlenecks in practical applications: first, insufficient activity, resulting in low conversion efficiency; second, poor selectivity, making it difficult to accurately control the generation of target products; third, insufficient stability, which is prone to performance degradation during long-term operation. These problems have seriously restricted the industrial application of Cu-based catalysts in the field of electrocatalytic CO2 reduction.

[0004] Therefore, in view of the deficiencies and shortcomings of the prior art, the present invention proposes a preparation method and application of a Cu-based catalyst with CeO2 as a carrier, which provides strong support for solving the current environmental pollution problem and promoting the recycling of carbon resources, and has significant social benefits and economic value. Summary of the invention

[0005] The purpose of the present invention is to make up for the shortcomings of the prior art and provide a preparation method and application of a Cu-based catalyst with CeO2 as a carrier. It synthesizes a rod-shaped CeO2 carrier with excellent performance by precisely controlling the hydrothermal reaction conditions, mixes and stirs the Cu precursor Cu(NO3)2 and the CeO2 carrier under different temperature conditions to ensure that Cu is evenly loaded on the carrier, and obtains a high-performance Cu / CeO2 catalyst after centrifugation, drying and calcination at 500°C for 4 hours. The catalyst shows significantly improved catalytic activity, selectivity and stability in the field of electrocatalytic carbon dioxide reduction, providing new ideas for research and application in related fields.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: On the one hand, a method for preparing a Cu-based catalyst using CeO2 as a carrier, the specific steps of the preparation method are:

[0007] Raw material preparation: Cu(NO3)2·3H2O was selected as the copper source, and pre-prepared cerium oxide CeO2 was used as the carrier material;

[0008] Solution preparation: Dissolve Cu salt and CeO2 in appropriate amount of water to form a uniform solution, slowly add salt solution to the solution, adjust the pH value to the appropriate range, and precipitate Cu ions in the form of carbonate or hydroxide;

[0009] Mixing and stirring: Mix the solution containing CeO2 with the above precipitate to form a mixed solution, and fully stir the mixed solution at different temperatures to explore the effects of different temperature conditions on the catalyst structure and performance;

[0010] Centrifugal drying: The stirred mixed solution is centrifuged to remove excess water and unabsorbed impurities, and the solid product after centrifugation is dried to obtain a preliminary Cu / CeO2 catalyst precursor;

[0011] Calcination treatment: The dried precursor is placed in a high-temperature furnace for calcination. During the calcination process, the Cu precursor is converted into CuO and firmly loaded on the surface of CeO2. At the same time, the CeO2 carrier also undergoes a certain degree of crystal transformation and structural optimization, further improving the catalytic activity and stability of the catalyst.

[0012] Furthermore, the solution is prepared by weighing a certain amount of Cu(NO3)2·3H2O crystals into a beaker, adding an appropriate amount of deionized water, placing it in an ultrasonic cleaner and ultrasonically dissolving it into a blue solution, weighing an appropriate amount of CeO2 powder into another beaker, adding deionized water and also ultrasonically forming a suspension, pouring the CeO2 suspension into the Cu(NO3)2 solution, stirring with a glass rod while pouring to make it evenly mixed, pouring the Na2CO3 solution into a dropping funnel, slowly opening the piston to add the Cu(NO3)2 solution drop by drop, monitoring with a precision pH meter during the dropwise addition, controlling the dropping speed to adjust the pH value to an appropriate range, so that the Cu ions are precipitated as carbonates or hydroxides.

[0013] Furthermore, the mixing and stirring is to carefully pour the solution containing CeO2 into the container containing the above-mentioned precipitate so that the two are in full contact to form a mixed liquid, and a portion of the mixed liquid is placed at room temperature and stirred with an electric stirrer, and another portion of the mixed liquid is placed in a constant temperature water bath, the water temperature is set, and the electric stirrer is also used for stirring, and a portion of the mixed liquid is placed in a refrigerator and continued to be stirred in a low temperature environment. During the stirring process under these three different temperature conditions, the stirring time must be long enough to ensure that the Cu precursor can be evenly distributed on the CeO2 surface.

[0014] Furthermore, the calcination process carefully places the dried precursor in a special crucible in a high-temperature furnace, sets the temperature of the high-temperature furnace to 500°C, and the time is 4 hours. The high-temperature furnace is started and the calcination operation begins. During the calcination, the Cu precursor will undergo chemical transformation and gradually turn into a Cu-based catalyst, which is firmly loaded on the CeO2 surface. After 4 hours of calcination, the high-temperature furnace is closed and the temperature in the furnace is allowed to cool naturally to room temperature.

[0015] Furthermore, the CeO2 carrier used is a rod-shaped structure, and the preparation method of the rod-shaped CeO2 is: mixing Ce(NO3)3 solution and NaOH solution, subjecting the mixed solution to a hydrothermal reaction, washing and drying, to obtain powdered cerium oxide.

[0016] Furthermore, the Ce(NO3)3 solution and the NaOH solution are mixed and stirred for 0.5h to form a reaction mixture, and the above mixture is placed in a polytetrafluoroethylene-lined hydrothermal reaction device for hydrothermal reaction at 100°C for 24 hours. After the reaction is completed, the supernatant is discarded and the precipitate is repeatedly washed with deionized water until it is neutral to remove residual impurities and ions. The washed precipitate is placed in an oven and dried at a suitable temperature to obtain powdered rod-shaped CeO2.

[0017] On the other hand, an application of a Cu-based catalyst with CeO2 as a carrier is characterized in that the Cu / CeO2 catalyst prepared by the above method can be applied to the field of electrocatalytic carbon dioxide reduction. By optimizing the composition and structure of the catalyst, the activity, selectivity and stability of carbon dioxide reduction are significantly improved, providing a new idea for the development of electrocatalytic carbon dioxide reduction technology.

[0018] Furthermore, the Cu-based catalyst with CeO2 as a carrier comprises: a Cu active component and a CeO2 carrier, wherein the Cu active component is uniformly loaded on the surface of the CeO2 carrier in the form of nanoparticles and uniformly distributed, and the CeO2 has a specific morphology and contains crystal faces of different proportions.

[0019] Furthermore, the role of the Cu-based catalyst with CeO2 as a carrier in the electrocatalytic reduction of carbon dioxide is that in terms of stabilization and enhancement of active sites, CeO2 can stabilize the Cu valence state by virtue of its unique electronic structure and redox properties, and in terms of catalytic performance optimization, it can significantly improve the product selectivity of CO2RR. In terms of structural and morphological effects, the different crystal faces and morphologies of the CeO2 carrier will significantly affect the catalytic performance of the Cu-based catalyst. In terms of catalytic mechanism and reaction path, the interaction between the CeO2 carrier and Cu can promote CO2 adsorption and activation, reduce the reaction energy barrier, accelerate the process, and can also regulate the reaction path by stabilizing the valence state and providing specific active sites, so that it tends to generate specific products.

[0020] Furthermore, the advantages of the Cu-based catalyst with CeO2 as the carrier in the electrocatalytic reduction of carbon dioxide are as follows: in terms of stabilization and enhancement of active sites, CeO2 can stabilize the Cu valence state by virtue of its unique electronic structure and redox properties; in terms of catalytic performance optimization, it can significantly improve the product selectivity of CO2RR; in terms of structural and morphological effects, the different crystal faces and morphologies of the CeO2 carrier will significantly affect the catalytic performance of the Cu-based catalyst; in terms of catalytic mechanism and reaction path, the interaction between the CeO2 carrier and Cu can promote CO2 adsorption and activation, reduce the reaction energy barrier, accelerate the process, and regulate the reaction path by stabilizing the valence state and providing specific active sites, so that it tends to generate specific products.

[0021] Compared with the prior art, the preparation method and application of the Cu-based catalyst using CeO2 as a carrier have the following beneficial effects:

[0022] 1. The present invention successfully loads Cu uniformly on CeO2 carriers with different crystal face ratios through a carefully designed preparation method. This unique structural design enables the catalyst to exhibit more excellent catalytic performance in the electrocatalytic carbon dioxide reduction process. The interaction between Cu and CeO2 not only enhances the catalyst's adsorption capacity for CO2, but also promotes the transfer of electrons and the stability of reaction intermediates, thereby significantly improving the activity of the catalyst. The different crystal face ratios of the CeO2 carrier provide diverse active sites for the reaction, further improving the catalyst's selectivity for the target product, making the product distribution more concentrated, which is beneficial to the subsequent purification and processing of products.

[0023] 2. The Cu / CeO2 catalyst of the present invention undergoes strict calcination treatment during the preparation process, which effectively improves the crystallinity and structural stability of the catalyst. This highly stable catalyst can maintain excellent catalytic activity during long-term operation of electrocatalytic carbon dioxide reduction and is not prone to deactivation or poisoning. The CeO2 carrier itself has excellent redox properties and can dynamically adjust its surface chemical state during the reaction, thereby enhancing the adaptability of the catalyst to reaction conditions. These characteristics enable the Cu / CeO2 catalyst of the present invention to have a longer service life and higher economic benefits in practical applications.

[0024] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 It is a measurement flow chart of a preparation method of a Cu-based catalyst using CeO2 as a carrier;

[0027] Figure 2 A scanning electron microscope image (SEM) of the CeO2 carrier prepared in the present invention;

[0028] Figure 3 X-ray diffraction spectrum (XRD) of Cu / CeO2 prepared by the present invention;

[0029] Figure 4 The electrocatalytic selectivity of Cu / CeO2 prepared by the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] Preparation of CeO2 carrier:

[0033] Prepare an appropriate amount of cerium nitrate precursor solution, place it in a clean container, and slowly add sodium hydroxide solution into it according to a specific stoichiometric ratio. During the addition process, use an electric stirrer to continuously stir for 0.5 hours to ensure that the two solutions are fully mixed.

[0034] After the mixing was completed, the obtained mixed solution was carefully transferred to a polytetrafluoroethylene-lined hydrothermal reaction device, and the temperature of the hydrothermal reaction was set to 100° C. and the reaction time was set to 24 hours.

[0035] After the hydrothermal reaction is completed, the reaction device is allowed to cool naturally to room temperature, the mixed liquid is taken out and placed in a centrifuge for centrifugal operation to separate the solid product. After the centrifugation is completed, the solid product is taken out and placed in a drying oven for drying to obtain the desired CeO2 carrier.

[0036] Configuration of Cu(NO3)2 solution:

[0037] Weigh a certain amount of Cu(NO3)2·3H2O and put it into a clean beaker. Use a measuring cylinder to measure an appropriate amount of deionized water and slowly pour it into the beaker. Place the beaker in an ultrasonic cleaner and turn on the ultrasonic function. Under the action of ultrasound, the Cu(NO3)2·3H2O crystals are completely dissolved and the solution is mixed evenly.

[0038] Configuration of Na2CO3 solution:

[0039] Accurately weigh a certain amount of Na2CO3 solid, put it into a clean beaker, use a measuring cylinder to measure an appropriate amount of deionized water and add it to the beaker, also put this beaker into an ultrasonic cleaner, use ultrasound to fully dissolve the Na2CO3 solid and mix the solution evenly.

[0040] Embodiment 2:

[0041] Preparation of Cu / CeO2 catalyst:

[0042] Weigh a certain amount of CeO2 powder, put it into a clean container, add an appropriate amount of water, and start the stirring device to evenly disperse the CeO2 powder in the water.

[0043] While continuing to stir, use a dropper to slowly add the Cu(NO3)2 solution to the above dispersion drop by drop. After adding, use an electric stirrer to keep stirring for 0.5 to 1 hour to ensure that the solution is fully mixed.

[0044] Next, continue to add Na2CO3 solution dropwise. After the addition is completed, extend the stirring time of the mixture to 6-7 hours to ensure that all components are fully reacted and evenly mixed.

[0045] For solutions mixed in a low temperature environment, if a stirring device is not available, the solution can be mixed evenly by gently shaking the container manually.

[0046] After the stirring is completed, the mixed solution is placed in a centrifuge for centrifugal operation to separate the solid matter, and then the solid matter obtained by centrifugation is dried to obtain the desired Cu / CeO2 catalyst.

[0047] Embodiment three:

[0048] CO2RR performance test of Cu / CeO2 catalyst:

[0049] Accurately weigh 10 mg of the prepared catalyst Cu / CeO2 powder and carefully place it in a clean container. Add a mixed solution of isopropanol and Nafion to the container, place the container in an ultrasonic cleaner, and start the ultrasonic function. Under the strong action of ultrasound, the catalyst powder is gradually dispersed in the mixed solution to form a uniform dispersion system. This ultrasonic process usually lasts 15-20 minutes to ensure the adequacy and uniformity of the dispersion.

[0050] From the dispersion after ultrasonic treatment, use a precision pipette to accurately absorb a certain amount of liquid, and evenly and slowly drop the absorbed dispersion on the surface of carbon paper with an area of ​​1×1 square centimeter. In order to ensure that the dispersion can evenly cover the surface of the carbon paper, the dropping speed and angle can be appropriately adjusted during the dropping process. After the dropping is completed, the carbon paper with the dispersion is placed in a well-ventilated and temperature-appropriate environment and allowed to dry naturally. The drying time is usually not less than 2 hours to ensure that the solvent is completely evaporated and the catalyst is firmly attached to the surface of the carbon paper.

[0051] When conducting performance tests, an H-cell device was used. A KHCO3 solution with a concentration of 0.1 mol / L was prepared in advance as the reaction liquid. Before the test began, pure CO2 gas was introduced into the reaction liquid at a steady flow rate for 0.5-1 hour. Such aeration treatment can fully dissolve CO2 in the reaction liquid, making it reach a saturated state, and provide a sufficient source of CO2 for subsequent reactions.

[0052] Subsequently, the fully dried carbon paper was installed in the H-cell device as the working electrode. At the same time, Ag / AgCl was selected as the reference electrode and the platinum mesh as the counter electrode. The test potential range was set to -1.6 to -1.8 volts relative to the reversible hydrogen electrode, and the performance of the catalyst was tested within this potential range.

[0053] During the entire test process, the generated gas products are analyzed and detected in real time by high-precision online chromatography equipment. The online chromatography can quickly and accurately separate and identify different gas components and quantitatively determine their concentrations. By analyzing the test results, the catalytic performance of the catalyst for the carbon dioxide reduction reaction at different potentials can be clearly understood, including the type of product, generation rate and key indicators of selectivity.

[0054] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a Cu-based catalyst using CeO2 as a carrier, characterized in that: The specific steps of the preparation method are: Raw material preparation: Cu(NO3)2·3H2O was selected as the copper source, and pre-prepared cerium oxide CeO2 was used as the carrier material; Solution preparation: Dissolve Cu salt and CeO2 in appropriate amount of water to form a uniform solution, slowly add salt solution to the solution, adjust the pH value to the appropriate range, and precipitate Cu ions in the form of carbonate or hydroxide; Mixing and stirring: Mix the solution containing CeO2 with the above precipitate to form a mixed solution, and fully stir the mixed solution at different temperatures to explore the effects of different temperature conditions on the catalyst structure and performance; Centrifugal drying: The stirred mixed solution is centrifuged to remove excess water and unabsorbed impurities, and the solid product after centrifugation is dried to obtain a preliminary Cu / CeO2 catalyst precursor; Calcination treatment: The dried precursor is placed in a high-temperature furnace for calcination. During the calcination process, the Cu precursor is converted into CuO and firmly loaded on the surface of CeO2. At the same time, the CeO2 carrier also undergoes a certain degree of crystal transformation and structural optimization, further improving the catalytic activity and stability of the catalyst.

2. The method for preparing a Cu-based catalyst using CeO2 as a carrier according to claim 1, characterized in that: The solution is prepared by weighing a certain amount of Cu(NO3)2·3H2O crystals into a beaker, adding an appropriate amount of deionized water, and placing the beaker in an ultrasonic cleaner to ultrasonically dissolve the crystals into a blue solution. An appropriate amount of CeO2 powder is weighed into another beaker, and deionized water is added and ultrasonically dissolved to form a suspension. The CeO2 suspension is poured into the Cu(NO3)2 solution, and stirred with a glass rod while pouring to make the mixture uniform. The Na2CO3 solution is poured into a dropping funnel, and the piston is slowly opened to dropwise add the Cu(NO3)2 solution. During the dropwise addition, a precision pH meter is used to monitor the pH value, and the dropping speed is controlled to adjust the pH value to an appropriate range so that the Cu ions are precipitated as carbonates or hydroxides.

3. The method for preparing a Cu-based catalyst with CeO2 as a carrier according to claim 1, characterized in that: The mixing and stirring process is to carefully pour the solution containing CeO2 into the container containing the above-mentioned precipitate so that the two are in full contact to form a mixed liquid. A portion of the mixed liquid is placed at room temperature and stirred with an electric stirrer. Another portion of the mixed liquid is placed in a constant temperature water bath, the water temperature is set, and the electric stirrer is also used for stirring. Another portion of the mixed liquid is placed in a refrigerator and continued to be stirred at a low temperature. During the stirring process under these three different temperature conditions, the stirring time must be long enough to ensure that the Cu precursor can be evenly distributed on the CeO2 surface.

4. The method for preparing a Cu-based catalyst using CeO2 as a carrier according to claim 1, characterized in that: The calcination treatment carefully places the dried precursor in a special crucible in a high-temperature furnace, sets the temperature of the high-temperature furnace to 500°C, and the time is 4 hours. The high-temperature furnace is started and the calcination operation begins. During the calcination, the Cu precursor will undergo chemical transformation and gradually turn into a Cu-based catalyst, which is firmly loaded on the CeO2 surface. After 4 hours of calcination, the high-temperature furnace is closed and the temperature in the furnace is allowed to cool naturally to room temperature.

5. The method for preparing a Cu-based catalyst with CeO2 as a carrier according to claim 1, characterized in that: The CeO2 carrier used is a rod-shaped structure. The preparation method of the rod-shaped CeO2 is: mixing a Ce(NO3)3 solution and a NaOH solution, subjecting the mixed solution to a hydrothermal reaction, washing and drying, and obtaining powdered cerium oxide.

6. The method for preparing a Cu-based catalyst using CeO2 as a carrier according to claim 5, characterized in that: The Ce(NO3)3 solution and the NaOH solution are mixed and stirred for 0.5h to form a reaction mixture. The mixture is placed in a hydrothermal reaction device lined with polytetrafluoroethylene and subjected to a hydrothermal reaction at 100°C for 24 hours. After the reaction, the supernatant is discarded and the precipitate is repeatedly washed with deionized water until it is neutral to remove residual impurities and ions. The washed precipitate is placed in an oven and dried at a suitable temperature to obtain powdered rod-shaped CeO2.

7. An application of a Cu-based catalyst with CeO2 as a carrier, characterized in that: The Cu / CeO2 catalyst prepared by the above method can be applied to the field of electrocatalytic carbon dioxide reduction. By optimizing the composition and structure of the catalyst, the activity, selectivity and stability of carbon dioxide reduction are significantly improved, providing new ideas for the development of electrocatalytic carbon dioxide reduction technology.

8. The use of a Cu-based catalyst with CeO2 as a carrier according to claim 7, characterized in that: The Cu-based catalyst with CeO2 as a carrier comprises: a Cu active component and a CeO2 carrier. The Cu active component is uniformly loaded on the surface of the CeO2 carrier in the form of nanoparticles and uniformly distributed. The CeO2 has a specific morphology and contains crystal faces of different proportions.

9. The use of a Cu-based catalyst with CeO2 as a carrier according to claim 7, characterized in that: The role of the Cu-based catalyst with CeO2 as a carrier in the electrocatalytic reduction of carbon dioxide is as follows: in terms of stabilization and enhancement of active sites, CeO2 can stabilize the Cu valence state by virtue of its unique electronic structure and redox properties; in terms of catalytic performance optimization, it can significantly improve the product selectivity of CO2RR; in terms of structure and morphology effects, different crystal faces and morphologies of the CeO2 carrier will significantly affect the catalytic performance of the Cu-based catalyst; in terms of catalytic mechanism and reaction path, the interaction between the CeO2 carrier and Cu can promote CO2 adsorption and activation, reduce the reaction energy barrier, accelerate the process, and can also regulate the reaction path by stabilizing the valence state and providing specific active sites, so that it tends to generate specific products.

10. The use of a Cu-based catalyst with CeO2 as a carrier according to claim 7, characterized in that: The advantages of the Cu-based catalyst with CeO2 as a carrier in the electrocatalytic reduction of carbon dioxide are as follows: in terms of stabilization and enhancement of active sites, CeO2 can stabilize the Cu valence state by virtue of its unique electronic structure and redox properties; in terms of catalytic performance optimization, it can significantly improve the product selectivity of CO2RR; in terms of structure and morphology effects, different crystal faces and morphologies of the CeO2 carrier will significantly affect the catalytic performance of the Cu-based catalyst; in terms of catalytic mechanism and reaction path, the interaction between the CeO2 carrier and Cu can promote CO2 adsorption and activation, reduce the reaction energy barrier, accelerate the process, and can also regulate the reaction path by stabilizing the valence state and providing specific active sites, so that it tends to generate specific products.

Citation Information

Cited By

  • Application of copper-loaded Ce-MOF derived cerium oxide carbon nanorod composite material in electrocatalytic reduction of Cr (VI)

    CN119797517A