Method for producing high-purity calcium phosphite by using by-product of sodium hypophosphite production

Through high-energy ball milling and micro-nano CO2 bubble reaction technology, the purity of calcium phosphate in the by-products produced by sodium hypophosphate is increased to 99.8%, solving the problems of low purity of calcium phosphate and complex process in the existing technology, achieving low purity of calcium phosphate in the existing technology Cost, green and environmentally friendly efficient preparation effect.

CN119018861APending Publication Date: 2024-11-26JIANGXI FUERXIN PHARM CHEM CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411084158.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The by-product of sodium hypophosphate produced by sodium hypophosphate has low purity and low yield, and the existing treatment methods are complex in the process and high in cost, and there are problems such as many impurities and low calcium and phosphorus recovery.

Method used

Nano-scale waste residue particles are formed by high-energy ball milling, dispersed in water by ultrasonic or stirring to form a suspension agent, and react with micro-nano CO2 bubbles to form calcium carbonate, and then react with excessive phosphoric acid, and then clean and dry to obtain high-purity calcium phosphite.

Benefits of technology

The preparation of high-purity calcium phosphite is achieved, with a purity of more than 99.8%, simple process, mild conditions, low cost, and no high temperature and high pressure requirements. It is suitable for large-scale industrial promotion, and is green and environmentally friendly, without pollution such as waste gas and waste acids. Things.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018861A_ABST
    Figure CN119018861A_ABST
Patent Text Reader

Abstract

The invention provides a method for producing high-purity calcium phosphite by using a by-product of sodium hypophosphite production. The method comprises the following steps: carrying out high-energy ball milling on the by-product, namely solid waste residue, of sodium hypophosphite production to form nanoscale waste residue particles; the nanoscale waste residue particles are dispersed in water through ultrasonic or stirring to form a uniform and stable suspension agent; the suspension agent reacts with the micro-nano CO2 bubbles, so that calcium hydroxide in the nano-scale waste residue particles reacts with CO2 to generate calcium carbonate; collecting precipitates in the reaction product and repeatedly cleaning; adding excessive phosphorous acid into the cleaned precipitate, and stirring to react, so that calcium carbonate reacts with phosphorous acid to generate calcium phosphite; and after solid-liquid separation, cleaning and drying the precipitate to obtain the high-purity calcium phosphite. According to the method disclosed by the invention, the solid waste residues in the by-products of sodium hypophosphite production are prepared into high-purity calcium phosphite through high-energy ball milling, homogeneous dispersion, carbonization and conversion reaction, and the purity is higher than 99.8%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial solid waste recycling, and particularly relates to a method for producing high-purity calcium phosphite by utilizing a byproduct of sodium hypophosphite production. Background Art

[0002] Sodium hypophosphite is an important industrial reducing agent, mainly used in chemical plating, electroplating, organic synthesis, food industry, etc. At present, sodium hypophosphite is mainly obtained by reacting yellow phosphorus with a mixture of calcium hydroxide and sodium hydroxide (or sodium carbonate), and a large amount of solid waste residue is also produced. According to statistics, 1 to 2 tons of industrial waste residue can be produced for every 1 ton of sodium hypophosphite produced. If it is not properly disposed, it will cause pollution to the ecological environment. According to measurements, the main components of industrial waste residues produced as a byproduct of sodium hypophosphite production are calcium phosphite, calcium hydroxide, calcium carbonate, and sodium hypophosphite, among which calcium phosphite has the largest content, and its weight proportion is generally higher than 30%, or even higher than 50%.

[0003] At present, the treatment methods of industrial waste residues generated by sodium hypophosphite production are mainly harmless and resource-based treatment, such as preparing phosphorous acid through ion exchange resin or electrolysis, or preparing calcium phosphate, phosphate fertilizer, etc. through high-temperature calcination.

[0004] However, due to the complex composition of industrial waste residues, when they are recycled to prepare other products, there will be problems such as more product impurities or low calcium and phosphorus recovery rates, or complex processes and high-cost, high-energy consumption operating steps are required.

[0005] Since the main component of waste residue is calcium phosphite, purifying industrial waste residue is one of the current ways to recycle waste residue. For example, the waste residue is subjected to sulfuric acid acid hydrolysis, resin ion exchange, palladium salt impurity removal, extraction, conversion and other processes to finally prepare high-purity calcium phosphite. The process is complicated, costly and will produce a large amount of sulfuric acid waste acid. Alternatively, phosphorous acid, calcium hydroxide, calcium oxide and other substances are directly added to the solid residue for reaction to obtain calcium phosphite. Studies have found that the purity of calcium phosphite prepared by the above methods is less than 99.5% and the yield is low. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a method for producing high-purity calcium phosphite using the by-product of sodium hypophosphite production, aiming to solve at least one technical problem among the background technology.

[0007] The present invention is achieved in that:

[0008] A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production comprises the following steps:

[0009] The byproduct (solid waste residue) of sodium hypophosphite production is subjected to high-energy ball milling to form nano-scale waste residue particles;

[0010] Nano-scale waste residue particles are dispersed in water by ultrasound or stirring to form a uniform and stable suspension;

[0011] The suspending agent reacts with the micro-nano CO2 bubbles, so that the calcium hydroxide in the nano-scale waste residue particles reacts with the CO2 to generate calcium carbonate; the precipitate in the reaction product is collected and repeatedly washed;

[0012] Add an excess of phosphorous acid to the washed precipitate and stir to react, so that calcium carbonate reacts with phosphorous acid to generate calcium phosphite; after solid-liquid separation, wash the precipitate, dry and dehydrate it to obtain high-purity calcium phosphite.

[0013] Furthermore, the step of reacting the suspending agent with the micro-nano CO2 bubbles specifically includes:

[0014] The suspension is placed in a sealed reaction device, and nitrogen is introduced to exhaust the air in the device;

[0015] Carbon dioxide and water are made into micro-nano CO2 bubbles and input from the bottom of the reaction equipment. The bicarbonate ions in the reaction equipment system are monitored. When bicarbonate ions appear, the reaction ends.

[0016] Furthermore, after the suspending agent reacts with the micro-nano CO2 bubbles, the following steps are also included: the reaction equipment is heated to 30°C to 40°C and then allowed to stand, and the residual carbon dioxide is discharged or collected in the form of gas.

[0017] Furthermore, the step of adding an excess of phosphorous acid to the washed precipitate and stirring the precipitate for reaction specifically comprises:

[0018] The cleaned precipitate is ground into slurry by adding water;

[0019] The slurry is placed in a reaction kettle, and an excess amount of phosphorous acid solution is added thereto;

[0020] The reaction is heated and stirred, and the carbon dioxide gas generated during the reaction is discharged.

[0021] Furthermore, the reaction is heated and stirred, and the reaction temperature after heating is 40°C to 60°C.

[0022] Furthermore, the D50 of the nano-scale waste residue particles is 30-50 nm.

[0023] Furthermore, the stirring speed is not less than 3000 rpm.

[0024] Furthermore, the introduction rate of the micro-nano CO2 bubbles is 50-100 mL / min.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention prepares high-purity calcium phosphite from solid waste residues in the by-product of sodium hypophosphite production through high-energy ball milling, homogeneous dispersion, carbonization, and conversion reactions, with a purity higher than 99.8%.

[0027] 2. The method of the present invention has simple procedures, mild conditions, does not require complex technical means such as high temperature and high pressure, and has low cost, which is conducive to large-scale industrial promotion.

[0028] 3. The method of the present invention is green and environmentally friendly, and does not produce pollutants such as waste gas and waste acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] The by-product of sodium hypophosphite production in the present application refers to solid waste residue. The by-product of the following embodiment is selected from the solid waste residue generated when Jiangxi Fuxin Pharmaceutical Chemical Co., Ltd. generates sodium hypophosphite. The synthesis process of sodium hypophosphite is as follows: first, quicklime and water are mixed in proportion to form lime slurry (calcium hydroxide emulsion), which is then pumped into a reactor, and then a certain amount of liquid alkali and yellow phosphorus are added to react. The phosphine produced during the reaction process is introduced into the gas cabinet through a water-sealed scrubber (washed in the next application), and the reaction liquid is filtered to obtain a crude sodium hypophosphite liquid. The crude liquid is purified (carbonization treatment), evaporated once, filtered once, adjusted pH once, filtered twice, adjusted pH twice, evaporated twice, crystallized, centrifuged, dried, packaged, and other processes to obtain a finished sodium hypophosphite product; the reaction formula in the synthesis process is:

[0032] CaO+H2O=Ca(OH)2

[0033] P4+3NaOH+6H2O=3NaH2PO2·H2O+PH3↑

[0034] P4+2Ca(OH)2+2H2O=2CaHPO3↓+2PH3↑

[0035] The filter residue produced in the above filtration process is the solid waste residue. Chemical analysis and energy spectrum analysis are performed on the solid waste residue to obtain the composition and content of the waste residue, as shown in Table 1.

[0036] Table 1

[0037]

[0038] The calcium carbonate in the solid waste is mainly derived from the reaction between sodium carbonate and calcium hydroxide during the pH adjustment of the crude liquid. Aluminum hydroxide, magnesium hydroxide and other impurities are all impurities derived from the reaction raw materials themselves.

[0039] A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production, the process is as follows Figure 1 As shown, the following steps are included:

[0040] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 30 to 50 nm;

[0041] S2, dispersing the nano-scale waste residue particles in water to form a uniform and stable suspension by ultrasound or stirring at a speed of not less than 3000 rpm;

[0042] S3, calcium hydroxide in the nano-scale waste slag particles reacts with CO2 to form calcium carbonate;

[0043] (1) placing the suspension in a sealed reaction device and introducing nitrogen to exhaust the air in the device;

[0044] (2) Carbon dioxide and water are made into micro-nano CO2 bubbles, and are introduced from the bottom of the reaction device, and bicarbonate ions in the reaction device system are monitored. When bicarbonate ions appear, the reaction ends; the diameter of the micro-nano CO2 bubbles is between 100 nanometers and 10 micrometers, and the average diameter is 0.1 to 10 μm; the introduction rate of the micro-nano CO2 bubbles is 50 to 100 mL / min;

[0045] (3) heating the reaction equipment to 30-40° C. and then allowing it to stand, and discharging or collecting the residual carbon dioxide in the form of gas;

[0046] (4) collecting and repeatedly washing the precipitate in the reaction product;

[0047] In this step, no additional stirring equipment is used to avoid destroying the morphology of the micro-nano CO2 bubbles and causing loss of their own characteristics.

[0048] S4, calcium carbonate reacts with phosphorous acid to generate calcium phosphite; specifically:

[0049] (1) adding water to the cleaned precipitate and grinding it into a slurry;

[0050] (2) placing the slurry in a reaction kettle and adding an excess of phosphorous acid solution thereto;

[0051] (3) heating to 40°C to 60°C and stirring for reaction, with the reactor equipped with a gas extraction device to discharge the generated carbon dioxide gas in real time during the reaction;

[0052] (4) After solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain high-purity calcium phosphite.

[0053] In the present invention, the function of step S1 is to form the solid waste into nano-scale powder with uniform particles, which not only makes the particle size finer, but also the frequent contact between the metal element powders during the mechanical high-energy ball milling process, and the continuous and intense plastic deformation makes the microstructure fine and uniform, which is conducive to the subsequent reaction.

[0054] The function of step S2 is to form a uniform and stable suspension of insoluble or poorly soluble objects in the solid waste residue based on external force, and the soluble or slightly soluble substances in the waste residue are efficiently dissolved in water, which is beneficial to subsequent separation;

[0055] The function of step S3 is to react CO2 with calcium hydroxide to generate calcium carbonate, and the reaction formula is: CO2+Ca(OH)2=CaCO3↓+H2O; if CO2 is excessive, it will continue to react to generate soluble calcium bicarbonate: H2O+CO2+CaCO3=Ca(HCO3)2; so online monitoring of bicarbonate ions is adopted, and when bicarbonate ions appear, the introduction of CO2 bubbles is stopped to terminate the reaction.

[0056] The main purpose of the reaction process in step S3 is: (1) to completely convert slightly soluble calcium hydroxide into insoluble calcium carbonate, thereby reducing calcium loss in the subsequent preparation of calcium phosphite. The conventional method is to first remove the sodium salt in the solid waste by washing with water, but in this process there will be calcium hydroxide dissolution loss. The present invention reacts calcium hydroxide with carbon dioxide to generate water-insoluble calcium carbonate, which effectively avoids calcium loss; (2) at the same time, magnesium impurities and the like are converted into slightly soluble carbonates, which can be initially separated and removed by filtration.

[0057] After solid-liquid separation (such as filtration) in step S3, the main components in the filtrate are sodium hypophosphite and some impurities; the main components of the solid precipitate are calcium phosphite and calcium carbonate. The role of subsequent heating and standing is to promote the discharge of excess carbon dioxide on the one hand, and to provide an environment for fixed sedimentation on the other hand. The temperature range setting ensures the effective overflow of carbon dioxide, while ensuring the operating environment safety of other instruments (such as bicarbonate ion detector). The flow rate of micro-nano CO2 bubbles is set to ensure the adequacy of the reaction. At the same time, if the flow rate is too slow, the reaction time is too long, resulting in unstable aggregation of the suspending agent and affecting the reaction efficiency.

[0058] In step S3, micro-nano CO2 bubbles are used to replace traditional CO2 gas for the following reasons: (1) The increased oxidizability of CO2 improves the reaction efficiency: When the micro-nano CO2 bubbles burst in the reaction equipment, the gas-liquid interface changes dramatically, and the high-concentration carbonate ions accumulated on the interface quickly release the accumulated chemical energy and promote the release of hydroxide ions in the suspending agent, so that metal ions such as calcium ions react quickly and efficiently with carbonate ions to form calcium carbonate. (2) The solubility of CO2 itself is increased: Compared with conventional carbon dioxide gas, micro-nano CO2 bubbles can make more carbon dioxide dissolve in water to form carbonic acid, thereby improving the reaction efficiency. (3) It can promote solid sedimentation: Since micro-nano CO2 bubbles have the characteristics of large specific surface area, it is easy to promote the agglomeration and sedimentation of the generated calcium carbonate.

[0059] The function of step S4 is to react calcium carbonate with phosphorous acid to generate calcium phosphite precipitate, CaCO3+H3PO3=CaHPO3↓+CO2↑++H2O, while promoting the dissolution of impurities such as calcium and magnesium in acid to facilitate subsequent removal.

[0060] The excess phosphorous acid in step S4 refers to the CaCO3 in the product of step S3 or to the Ca(OH)2 and CaCO3 in the solid waste, that is, the amount of phosphorous acid added (molar amount) is equal to the CaCO3 in the product of step S3 according to the theoretical amount, and is slightly higher than the theoretical amount by about 10% in practical applications. On the one hand, it is to ensure the sufficiency of the reaction, and on the other hand, it provides an acidic environment for the dissolution of impurities such as calcium and magnesium.

[0061] After solid-liquid separation (such as filtration) in step S4, the main component in the filtrate is a dilute phosphorous acid solution, and the solid precipitate is high-purity calcium phosphite.

[0062] In step S4, the washed precipitate is processed into a slurry before the reaction because it is more conducive to the reaction of calcium carbonate and phosphorous acid and improves the reaction efficiency; at the same time, carbon dioxide is discharged in real time during the reaction, which is conducive to the forward reaction. During the reaction, the temperature is controlled at 50°C to 100°C, on the one hand to promote the reaction efficiency, and on the other hand to promote the discharge of carbon dioxide; in addition, this temperature range can ensure the safety of the reactor and the stability of phosphorous acid.

[0063] The carbon dioxide gas discharged in steps S3 and S4 can be recycled and reused to prepare micro-nano CO2 bubbles; the filtrate after solid-liquid separation in step S3 mainly consists of sodium hypophosphite, which can be recycled as a mother liquor for preparing high-purity sodium hypophosphite; the filtrate after solid-liquid separation in step S3 mainly consists of phosphorous acid, which can also be recycled and reused.

[0064] Example 1

[0065] A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production comprises the following steps:

[0066] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 30 nm;

[0067] S2, dispersing 100g of nano-scale waste residue particles in 250mL of water by ultrasound to form a uniform and stable suspension, the ultrasonic parameters are 200W, 65KHz, and the time is 5min;

[0068] S3, dry ice and water are made into micro-nano CO2 bubbles with a diameter between 100 nanometers and 10 micrometers under the action of a micro-nano bubble generator, and the micro-nano CO2 bubbles are sealed and connected to the bottom of the reaction device; the suspending agent is placed in the sealed reaction device, and nitrogen is introduced to exhaust the air in the device; during the reaction, micro-nano CO2 bubbles are input from the bottom of the reaction device at a rate of 70 mL / min, and the calcium hydroxide in the solid waste reacts with CO2 to generate calcium carbonate; a bicarbonate ion detector is installed in the reaction device to monitor in real time whether bicarbonate ions are generated in the reaction device system, and the reaction is terminated when bicarbonate ions appear; after the reaction is completed, the reaction is heated to 30°C and then allowed to stand for about 1 hour, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0069] S4. Grind the washed precipitate into slurry by adding water; place the slurry in a reactor, and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 50°C and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain high-purity calcium phosphite.

[0070] Example 2

[0071] A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production comprises the following steps:

[0072] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 40 nm;

[0073] S2, dispersing 100g of nano-scale waste residue particles in 250mL of water by ultrasound to form a uniform and stable suspension, the ultrasonic parameters are 200W, 65KHz, and the time is 5min;

[0074] S3, dry ice and water are made into micro-nano CO2 bubbles with a diameter between 100 nanometers and 10 micrometers under the action of a micro-nano bubble generator, and the micro-nano CO2 bubbles are sealed and connected to the bottom of the reaction device; a suspending agent is placed in a sealed reaction device, and nitrogen is introduced to exhaust the air in the device; during the reaction, micro-nano CO2 bubbles are input from the bottom of the reaction device at a rate of 50 mL / min, and calcium hydroxide in the solid waste reacts with CO2 to generate calcium carbonate; a bicarbonate ion detector is installed in the reaction device to monitor in real time whether bicarbonate ions are generated in the reaction device system, and the reaction is terminated when bicarbonate ions appear; after the reaction is completed, the reaction is heated to 40°C and allowed to stand for about 1 hour, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0075] S4. Grind the washed precipitate with water to form a slurry; place the slurry in a reactor and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 40°C and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain a solid product - high-purity calcium phosphite.

[0076] Example 3

[0077] A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production comprises the following steps:

[0078] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 50 nm;

[0079] S2, dispersing 100 g of nano-scale waste residue particles in 250 mL of water by high-speed stirring at 5000 rpm to form a uniform and stable suspension;

[0080] S3, dry ice and water are made into micro-nano CO2 bubbles with a diameter between 100 nanometers and 10 micrometers under the action of a micro-nano bubble generator, and the micro-nano CO2 bubbles are sealed and connected to the bottom of the reaction device; a suspending agent is placed in a sealed reaction device, and nitrogen is introduced to discharge the air in the device; during the reaction, micro-nano CO2 bubbles are input from the bottom of the reaction device at a rate of 100 mL / min, and calcium hydroxide in the solid waste reacts with CO2 to generate calcium carbonate; a bicarbonate ion detector is installed in the reaction device to monitor in real time whether bicarbonate ions are generated in the reaction device system, and the reaction is terminated when bicarbonate ions appear; after the reaction is completed, the reaction is heated to 50°C and allowed to stand for about 1 hour, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0081] S4. Grind the washed precipitate with water to form a slurry; place the slurry in a reactor and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 60° C. and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain a solid product - high-purity calcium phosphite.

[0082] Comparative Example 1

[0083] This comparative example 1 is a method for producing calcium phosphite using the byproduct of sodium hypophosphite production, which differs from Example 1 in that step S1 is omitted and comprises the following steps:

[0084] S1. Disperse 100 g of solid waste residue produced as a byproduct of sodium hypophosphite production in 250 mL of water by ultrasound to form a uniform and stable suspension, with the ultrasonic parameters being 200 W, 65 KHz, and the time being 15 min;

[0085] S2, dry ice and water are made into micro-nano CO2 bubbles with a diameter between 100 nanometers and 10 micrometers under the action of a micro-nano bubble generator, and the micro-nano CO2 bubbles are sealed and connected to the bottom of the reaction device; a suspending agent is placed in a sealed reaction device, and nitrogen is introduced to exhaust the air in the device; during the reaction, micro-nano CO2 bubbles are input from the bottom of the reaction device at a rate of 70 mL / min, and calcium hydroxide in the solid waste reacts with CO2 to generate calcium carbonate; a bicarbonate ion detector is installed in the reaction device to monitor in real time whether bicarbonate ions are generated in the reaction device system, and the reaction is terminated when bicarbonate ions appear; after the reaction is completed, the reaction is heated to 30°C and then allowed to stand for about 1 hour, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0086] S3. Grind the washed precipitate into slurry by adding water; place the slurry in a reactor and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 50°C and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain a solid product.

[0087] Comparative Example 2

[0088] Comparative Example 2 is a method for producing calcium phosphite using the byproduct of sodium hypophosphite production. The difference between the method and Example 1 is that CO2 gas is directly introduced into step S3 instead of micro-nano CO2 bubbles, and the method comprises the following steps:

[0089] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 30 nm;

[0090] S2, dispersing 100g of nano-scale waste residue particles in 250mL of water by ultrasound to form a uniform and stable suspension, the ultrasonic parameters are 200W, 65KHz, and the time is 5min;

[0091] S3, placing the suspending agent in a sealed reaction device, and introducing nitrogen to exhaust the air in the device; during the reaction, CO2 gas is input from the bottom of the reaction device at 70mL / min, and the calcium hydroxide in the solid waste reacts with CO2 to form calcium carbonate; the reaction time is the same as that in Example 1; after the reaction is completed, it is heated to 30°C and allowed to stand for about 1h, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0092] S4. Grind the washed precipitate into slurry by adding water; place the slurry in a reactor and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 50°C and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain a solid product.

[0093] Comparative Example 3

[0094] This comparative example 3 is a method for producing calcium phosphite using the byproduct of sodium hypophosphite production, which differs from Example 1 in that step S3 is omitted and comprises the following steps:

[0095] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 30 nm;

[0096] S2, dispersing 100g of nano-scale waste residue particles in 250mL of water by ultrasound to form a uniform and stable suspension, the ultrasonic parameters are 200W, 65KHz, and the time is 5min;

[0097] S3. Place the suspending agent in a reactor and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 50°C and stir to react. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain a solid product.

[0098] Comparative Example 4

[0099] Comparative Example 4 is a method for producing calcium phosphite using a byproduct of sodium hypophosphite production, which differs from Example 1 in that step S2 comprises the following steps:

[0100] S1, high-energy ball milling of waste residues, a byproduct of sodium hypophosphite production, to form nano-scale waste residue particles with a D50 of 30 nm;

[0101] S2, stirring and mixing 100 g of nano-scale waste residue particles with 250 mL;

[0102] S3, dry ice and water are made into micro-nano CO2 bubbles with a diameter between 100 nanometers and 10 micrometers under the action of a micro-nano bubble generator, and the micro-nano CO2 bubbles are sealed and connected to the bottom of the reaction device; the suspending agent is placed in the sealed reaction device, and nitrogen is introduced to exhaust the air in the device; during the reaction, micro-nano CO2 bubbles are input from the bottom of the reaction device at a rate of 70 mL / min, and the calcium hydroxide in the solid waste reacts with CO2 to generate calcium carbonate; a bicarbonate ion detector is installed in the reaction device to monitor in real time whether bicarbonate ions are generated in the reaction device system, and the reaction is terminated when bicarbonate ions appear; after the reaction is completed, the reaction is heated to 30°C and then allowed to stand for about 1 hour, and the residual carbon dioxide is discharged or collected in the form of gas; the precipitate in the reaction product is collected and washed with clean water;

[0103] S4. Grind the washed precipitate into slurry by adding water; place the slurry in a reactor, and add an excess of 0.5 mol / L phosphorous acid solution (about 100 mL) thereto; heat to 50°C and stir the reaction for about 1 hour. During the reaction, the carbon dioxide gas generated is discharged, and after solid-liquid separation, the precipitate is washed, dried and dehydrated to obtain high-purity calcium phosphite.

[0104] The solid products finally obtained in Examples 1 to 3 and Comparative Examples 1 to 4 were weighed, and their components were analyzed by gas chromatography-mass spectrometry. The results are shown in Table 2.

[0105] Table 2

[0106]

[0107]

[0108] The yield is calculated based on the molar amount of calcium in the solid waste.

[0109] It can be seen from Table 2 above that the solid product prepared in the embodiments of the present invention contains high-purity calcium phosphite, and the purity is basically above 99.8%.

[0110] In Comparative Example 1, the unmilled solid waste residue was dispersed, carbonized and reacted with phosphorous acid. It can be seen that although the final product yield is high, the purity of calcium phosphite in the product is not high. After testing, it is found that there are also calcium hydroxide, calcium carbonate and other impurities. The reason is that the conventional solid waste residue particles are large. In the subsequent reaction process, the reaction progress is slow and the efficiency is low, resulting in calcium hydroxide and calcium carbonate not reacting with phosphorous acid.

[0111] Comparative Example 2 uses carbon dioxide gas as the raw material for the carbonization process, which makes the carbonization reaction efficiency low. On the one hand, it causes part of the calcium hydroxide to dissolve in water during the subsequent solid-liquid separation, causing calcium loss, so the yield of the product is reduced. On the other hand, a large amount of calcium hydroxide does not react, and the pH value of the reaction liquid increases during the subsequent conversion reaction, which is not conducive to the dissolution and removal of impurities such as magnesium and aluminum, resulting in a slightly lower purity than Example 1.

[0112] In Comparative Example 3, the carbonization procedure was deleted, and the final product was found to contain calcium hydroxide, calcium carbonate and other impurities. The reason is that the conventional conversion reaction is inefficient and time-consuming, and calcium hydroxide and calcium carbonate do not have enough time to be converted into calcium phosphite, resulting in reduced purity.

[0113] In Comparative Example 4, the dispersion method in step S2 is deleted, and conventional mixing is directly adopted. Since most of the solid waste residue is substances that are insoluble or difficult to dissolve in water, solid-liquid stratification occurs, which is not conducive to subsequent carbonization and conversion reactions. Therefore, the final product is tested to have a small amount of calcium hydroxide and calcium carbonate, and the purity is low.

[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production, characterized in that: The byproduct of the sodium hypophosphite production is solid waste residue, and the method comprises the following steps: High-energy ball milling of solid waste residues to form nano-scale waste residue particles; Nano-scale waste residue particles are dispersed in water by ultrasound or stirring to form a uniform and stable suspension; The suspending agent reacts with the micro-nano CO2 bubbles, so that the calcium hydroxide in the nano-scale waste residue particles reacts with the CO2 to generate calcium carbonate; the precipitate in the reaction product is collected and repeatedly washed; Add an excess of phosphorous acid to the washed precipitate and stir to react, so that calcium carbonate reacts with phosphorous acid to generate calcium phosphite; after solid-liquid separation, wash the precipitate, dry and dehydrate it to obtain high-purity calcium phosphite.

2. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 1, characterized in that: The step of reacting the suspending agent with the micro-nano CO2 bubbles specifically includes: The suspension is placed in a sealed reaction device, and nitrogen is introduced to exhaust the air in the device; Carbon dioxide and water are made into micro-nano CO2 bubbles and input from the bottom of the reaction equipment. The bicarbonate ions in the reaction equipment system are monitored. When bicarbonate ions appear, the reaction ends.

3. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 2, characterized in that: After the suspension reacts with the micro-nano CO2 bubbles, the following steps are also included: heating the reaction equipment to 30°C to 40°C and then letting it stand, and discharging or collecting the residual carbon dioxide in the form of gas.

4. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 1, characterized in that: The step of adding an excess of phosphorous acid to the washed precipitate and stirring the mixture for reaction specifically comprises: The cleaned precipitate is ground into slurry by adding water; The slurry is placed in a reaction kettle, and an excess amount of phosphorous acid solution is added thereto; The reaction is heated and stirred, and the carbon dioxide gas generated during the reaction is discharged.

5. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 4, characterized in that: The reaction temperature after heating is 40°C to 60°C.

6. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 1, characterized in that: The D50 of the nano-scale waste residue particles is 30-50 nm.

7. A method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 1, characterized in that: The stirring speed is not less than 3000 rpm.

8. The method for producing high-purity calcium phosphite using a byproduct of sodium hypophosphite production according to claim 1, characterized in that: The introduction amount of the micro-nano CO2 bubbles is 50-100 mL / min.

Citation Information

Cited By

  • Treatment process of by-product sodium hypophosphite in phosphorane preparation process

    CN120757084A

  • Method for preparing phosphorane through pyrolysis of sodium hypophosphite based on raw material pretreatment

    CN120793858A