Preparation method of metal ion-doped modified iron oxide composite pigment

By doping metal ions and using additives in the iron oxide pigment to form a solid solution, the problem of insufficient temperature resistance of the iron oxide pigment is solved, and the uniform color and temperature resistance are improved, and the cost is reduced.

CN119019865APending Publication Date: 2024-11-26YIXING YUXING IND & TRADE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121394.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The temperature resistance of iron oxide pigments is insufficient, resulting in color changes and color loss in low or high temperature environments. The existing improvement methods require the selection and adjustment of additives according to actual conditions, which is relatively expensive.

Method used

Iron oxide red is prepared by doping different metal ions (such as manganese, cobalt, vanadium, copper and zinc) into the iron oxide components and adding additives such as fillers and consistency regulators, and grinding, filtering and drying. Compound pigments to form solid solution to improve thermal stability and temperature resistance.

Benefits of technology

The temperature resistance and thermal stability of iron oxide pigments are significantly improved, metal ion agglomeration is avoided, and the pigments obtained are uniform in color and excellent in temperature resistance, reducing the actual application cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a metal ion-doped modified iron oxide composite pigment, and belongs to the field of modification and preparation of inorganic pigments. Metal ions such as manganese, cobalt, vanadium, copper, zinc and the like are mixed with the iron oxide pigment, then related auxiliaries such as the adhesive and the like are added for tempering and aging, the reaction activity of all metal components can be improved, combination of all the components can be achieved, finally, the consistency of the slurry can be well adjusted by supplementing the consistency adjusting agent, and therefore the corrosion resistance of the slurry is improved. The agglomeration phenomenon of metal ions caused by overlarge consistency is avoided, and finally the iron oxide composite pigment with uniform color, relatively good chromaticity and excellent temperature resistance is obtained. In the preparation process of the iron oxide pigment, the crystal structure of the pigment is more regular by doping metal ions such as manganese, cobalt, vanadium, copper and zinc, adding related auxiliaries such as a filler and controlling parameters such as reaction time, temperature and pressure, and the thermal stability and temperature resistance of the iron oxide pigment can be improved by forming a solid solution of iron oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of modification and preparation of inorganic pigments, and in particular relates to a method for preparing a composite iron oxide pigment modified by doping metal ions. Background Art

[0002] Iron oxide red pigment is a common pigment with excellent properties such as weather resistance, light resistance, corrosion resistance, and strong tinting power. It is widely used in construction, paint, printing and dyeing, plastics, etc. However, there are also some problems when using this pigment. One of the important problems is that it is not heat resistant enough, and it often changes color or loses color due to the effect of low or high temperature environment.

[0003] At present, in order to solve the temperature resistance of iron oxide pigments, it is usually started from the preparation process of iron oxide pigments or by adding additives to improve the temperature resistance of iron oxide pigments. From the process aspect, the temperature resistance of iron oxide yellow pigments can be improved mainly by adjusting the processing technology when manufacturing pigments to improve the temperature resistance of iron oxide yellow pigments. For example, in the process of preparing iron oxide yellow pigments, the reaction time, temperature and pressure are controlled to make the crystal structure of the pigment more regular, thereby improving its temperature resistance. Adding additives is also one of the effective means to improve the temperature resistance of iron oxide yellow pigments. Common additives include metal ions such as zinc, cobalt, copper, nickel and zirconium. These additives can react with iron oxide components to improve the thermal stability and temperature resistance of iron oxide yellow pigments. However, the use and precautions of additives need to be determined according to the actual situation. Generally speaking, the additive powder and iron oxide red pigment are mixed evenly, and then added to other coating raw materials for mixing. When using additives, the following matters should also be noted: First, the additives should not be excessive, otherwise the color and performance of the pigment may change. Secondly, the selection of additives needs to comprehensively consider factors such as pigment properties, production process and cost to select appropriate additives.

[0004] The above methods can improve the thermal stability and temperature resistance of iron oxide red pigment, so that it can be better applied in various occasions. However, in actual preparation or modification, it is necessary to select and adjust the additives according to the actual situation and needs to obtain the best effect. Therefore, in order to further improve the temperature resistance and thermal stability of iron oxide pigment, it is urgent to develop a new formula and type of additives to improve the temperature resistance and thermal stability of iron oxide pigment and reduce the cost of actual application of iron oxide pigment. Summary of the invention

[0005] In order to solve the above technical problems, the present invention discloses a preparation method of a metal ion-doped modified iron oxide pigment, which comprises doping different metal ions on the basis of the original iron oxide component, mixing and grinding, adding relevant auxiliary agents for tempering and aging, and obtaining an iron oxide red composite pigment after filter pressing, powdering and sieving.

[0006] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0008] Step 1, weighing 3 to 5 parts of calcined diatomaceous earth, 2 to 3 parts of calcined kaolin, 1 to 2 parts of mica powder, 15 to 25 parts of zinc oxide, 5 to 12 parts of manganese dioxide, 3 to 8 parts of cobalt oxide, 5 to 9 parts of vanadium pentoxide, 8 to 15 parts of copper oxide and 55 to 85 parts of iron oxide in a container, and stirring and mixing;

[0009] Step 2, adding water, a dispersant and a binder into a container, heating and stirring to prepare a mixed slurry;

[0010] Step 3, grinding the mixed slurry obtained in step 2, adding a filler and a consistency regulator, and letting it stand;

[0011] Step 4, filtering, drying, powdering and sieving the mixed material after standing in step 3 to obtain a metal ion-doped modified iron oxide composite pigment.

[0012] Furthermore, in step 1, the components weighed in parts by weight are: 3 parts of calcined diatomaceous earth, 2 parts of calcined kaolin, 1 part of mica powder, 15 parts of zinc oxide, 12 parts of manganese dioxide, 3 parts of cobalt oxide, 9 parts of vanadium pentoxide, 12 parts of copper oxide and 85 parts of iron oxide.

[0013] Furthermore, in step 2, the added amounts of water, dispersant and binder are 100-200%, 0.1-0.3% and 2.0-3.0% of the total mass of the mixed material, respectively.

[0014] Furthermore, in step 2, the added amounts of water, dispersant and binder are 180%, 0.3% and 2.0% of the total mass of the mixed material, respectively.

[0015] Furthermore, in step 2, the dispersant is selected from one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate; and the binder is sodium silicate.

[0016] Furthermore, in step 2, the temperature of heating and stirring is 65-80°C.

[0017] Furthermore, in step 3, the added amounts of the filler and consistency regulator are 0.5-0.8% and 0.3-0.5% of the total weight of the mixed material, respectively.

[0018] Furthermore, the filler is sodium metasilicate; and the consistency regulator is polyethylene glycol.

[0019] Furthermore, in step 4, the drying is carried out by oven drying until the moisture content does not exceed 0.5%.

[0020] Furthermore, the metal ion-doped modified iron oxide composite pigment is prepared by any of the above methods.

[0021] Beneficial effects: Compared with the prior art, the advantages of the present invention include:

[0022] (1) In the process of preparing the iron oxide pigment, the present invention makes the crystal structure of the pigment more regular by doping other metal ions and controlling parameters such as reaction time, temperature and pressure, thereby improving the temperature resistance.

[0023] (2) The present invention dopes the original iron oxide pigment components with metal ions such as manganese, cobalt, vanadium, copper and zinc and adds relevant additives such as fillers, which can improve the thermal stability and temperature resistance of the iron oxide pigment by forming a solid solution of iron oxide, especially Mn 2+ and Cu 2+ The introduction of can significantly improve the heat resistance of iron oxide pigments.

[0024] (3) The present invention first mixes other metal ions with the iron oxide pigment, and then adds adhesives and other related additives for tempering and aging, which can not only enhance the reactivity of each metal component, but also achieve the combination of each component. Finally, by adding a consistency regulator, the slurry consistency can be well adjusted to avoid the agglomeration of metal ions caused by excessive consistency, and finally obtain an iron oxide composite pigment with uniform color, good chroma and excellent temperature resistance. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0026] Unless otherwise specified, the raw materials or reagents used in the following examples are all commercially available products; unless otherwise specified, the methods used to test the products are all commonly used detection methods in the art.

[0027] The technical solutions of various embodiments of the present invention are described in detail below using red iron oxide as an example.

[0028] Example 1

[0029] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0030] (1) 3 to 5 parts of calcined diatomaceous earth, 2 to 3 parts of calcined kaolin, 1 to 2 parts of mica powder, 15 to 25 parts of zinc oxide, 5 to 12 parts of manganese dioxide, 3 to 8 parts of cobalt oxide, 5 to 9 parts of vanadium pentoxide, 8 to 15 parts of copper oxide and 55 to 85 parts of iron oxide are weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 30 to 45 minutes to obtain a mixed material;

[0031] (2) adding water, a dispersant and sodium silicate to the mixture obtained in step (1), heating to 65-80° C., mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, dispersant (sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate) and binder (sodium silicate) added is 100-200%, 0.1-0.3% and 2.0-3.0% of the total mass of the mixture, respectively;

[0032] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.5 to 0.8% of filler (sodium metasilicate) and 0.3 to 0.5% of consistency regulator (polyethylene glycol) to the ground mixed slurry, stirring evenly, and standing for 2 to 3 hours;

[0033] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, powdered, and sieved to obtain an iron oxide red composite pigment.

[0034] Example 2

[0035] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0036] (1) 3 parts of calcined diatomaceous earth, 2 parts of calcined kaolin, 1 part of mica powder, 15 parts of zinc oxide, 12 parts of manganese dioxide, 3 parts of cobalt oxide, 9 parts of vanadium pentoxide, 12 parts of copper oxide and 85 parts of iron oxide were weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 45 minutes to obtain a mixed material;

[0037] (2) adding water, sodium tripolyphosphate and sodium silicate to the mixture obtained in step (1), mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium tripolyphosphate and sodium silicate added is 180%, 0.3% and 2.0% of the total mass of the mixture, respectively;

[0038] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.8% sodium metasilicate and 0.5% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for aging for 3 hours;

[0039] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, and then powdered and sieved to obtain an iron oxide red composite pigment.

[0040] Example 3

[0041] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0042] (1) Weigh 4 parts by weight of calcined diatomaceous earth, 3 parts by weight of calcined kaolin, 2 parts by weight of mica powder, 15 parts by weight of zinc oxide, 12 parts by weight of manganese dioxide, 5 parts by weight of cobalt oxide, 9 parts by weight of vanadium pentoxide, 10 parts by weight of copper oxide and 80 parts by weight of iron oxide into a container with a stirring and grinding function, and stir for 45 minutes to obtain a mixed material;

[0043] (2) adding water, sodium hexametaphosphate and sodium silicate to the mixture obtained in step (1), mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium hexametaphosphate and sodium silicate added is 200%, 0.2% and 3.0% of the total mass of the mixture, respectively;

[0044] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.6% sodium metasilicate and 0.3% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for 2 hours;

[0045] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, and then powdered and sieved to obtain an iron oxide red composite pigment.

[0046] Example 4

[0047] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0048] (1) 3 parts of calcined diatomite, 2 parts of calcined kaolin, 1 part of mica powder, 20 parts of zinc oxide, 10 parts of manganese dioxide, 8 parts of cobalt oxide, 5 parts of vanadium pentoxide, 15 parts of copper oxide and 70 parts of iron oxide were weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 40 minutes to obtain a mixed material;

[0049] (2) adding water, sodium pyrophosphate and sodium silicate to the mixture obtained in step (1), mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium pyrophosphate and sodium silicate added is 150%, 0.1% and 2.0% of the total mass of the mixture, respectively;

[0050] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.5% sodium metasilicate and 0.3% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for aging for 2 hours;

[0051] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, and then powdered and sieved to obtain an iron oxide red composite pigment.

[0052] Example 5

[0053] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0054] (1) Weigh 4 parts by weight of calcined diatomaceous earth, 3 parts by weight of calcined kaolin, 2 parts by weight of mica powder, 25 parts by weight of zinc oxide, 8 parts by weight of manganese dioxide, 3 parts by weight of cobalt oxide, 7 parts by weight of vanadium pentoxide, 15 parts by weight of copper oxide and 85 parts by weight of iron oxide into a container with a stirring and grinding function, and stir for 45 minutes to obtain a mixed material;

[0055] (2) adding water, sodium tripolyphosphate and sodium silicate to the mixture obtained in step (1), mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium tripolyphosphate and sodium silicate added is 200%, 0.3% and 3.0% of the total mass of the mixture, respectively;

[0056] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.8% sodium metasilicate and 0.5% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for 2 hours;

[0057] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, and then powdered and sieved to obtain an iron oxide red composite pigment.

[0058] Example 6

[0059] A method for preparing a metal ion-doped modified iron oxide composite pigment comprises the following steps:

[0060] (1) 3 parts of calcined diatomaceous earth, 2 parts of calcined kaolin, 1 part of mica powder, 15 parts of zinc oxide, 5 parts of manganese dioxide, 5 parts of cobalt oxide, 7 parts of vanadium pentoxide, 8 parts of copper oxide and 85 parts of iron oxide were weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 45 minutes to obtain a mixed material;

[0061] (2) adding water, sodium tripolyphosphate and sodium silicate to the mixture obtained in step (1), mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium tripolyphosphate and sodium silicate added is 180%, 0.2% and 3.0% of the total mass of the mixture, respectively;

[0062] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.6% sodium metasilicate and 0.5% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for aging for 2 hours;

[0063] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, and then powdered and sieved to obtain an iron oxide red composite pigment.

[0064] Comparative Example 1

[0065] Commercially available red iron oxide products are not modified by any metal doping or related additives.

[0066] Comparative Example 2

[0067] A preparation method of a metal ion-doped modified iron oxide pigment, comprising the following steps:

[0068] (1) 10 parts of zinc oxide, 3 parts of manganese dioxide, 2 parts of cobalt oxide, 2 parts of vanadium pentoxide, 5 parts of copper oxide and 85 parts of iron oxide were weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 45 minutes to obtain a mixed material;

[0069] (2) adding water, a dispersant and sodium silicate to the mixture obtained in step (1), heating to 80° C., mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium tripolyphosphate and sodium silicate added is 200%, 0.1% and 3.0% of the total mass of the mixture, respectively;

[0070] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.5% sodium metasilicate and 0.3% polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for aging for 2 hours;

[0071] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, powdered, and sieved to obtain an iron oxide red composite pigment.

[0072] Comparative Example 3

[0073] A preparation method of a metal ion-doped modified iron oxide pigment, comprising the following steps:

[0074] (1) 30 parts of zinc oxide, 15 parts of cobalt oxide, 5 parts of vanadium pentoxide, 15 parts of copper oxide and 85 parts of iron oxide are weighed respectively by weight and added into a container with a stirring and grinding function, and stirred for 30 to 45 minutes to obtain a mixed material;

[0075] (2) adding water, a dispersant and sodium silicate to the mixture obtained in step (1), heating to 80° C., mixing, stirring and grinding to prepare a mixed slurry; wherein the amount of water, sodium tripolyphosphate and sodium silicate added is 200%, 0.3% and 3.0% of the total mass of the mixture, respectively;

[0076] (3) grinding the mixed slurry obtained in step (2) to make the average particle size of the ground material 1 to 50 μm, adding 0.5% of sodium metasilicate and 0.5% of polyethylene glycol based on the total weight of the mixed material to the ground mixed slurry, stirring evenly, and standing for aging for 3 hours;

[0077] (4) The mixed material aged in step (3) is filtered through a plate and frame filter press to obtain a filter cake, and the filter cake is dried to a moisture content of less than 0.5%, powdered, and sieved to obtain an iron oxide red composite pigment.

[0078] The heat resistance performance of the iron oxide red composite pigments prepared in the above-mentioned embodiments 2 to 6 and comparative examples 1 to 3 was tested respectively; the test method is: a. Weigh 8.0g of the obtained iron oxide red composite pigment, put it into an oven at 400°C and bake it evenly for 25 to 30 minutes, and take it out for use after it is naturally cooled to room temperature; b. Weigh 2.5g of the iron oxide red samples before and after baking, add 0.5g of zinc oxide respectively and mix evenly, and then add 2.5mL of ink oil respectively to apply the sample on a transparent glass plate to form a uniform ink slurry layer until the ink slurry is coated into a film layer with a thickness of 100μm; c. Use a colorimeter to measure the color values ​​CIELAB of the two film layers, calculate the change ΔE of CIELAB, and use the size of ΔE to measure the heat resistance. The smaller the ΔE, the better the heat resistance. The test results are shown in Table 1 below. Table 1 Comparison of the heat resistance performance of the iron oxide red composite pigments prepared in Examples 2 to 6 and Comparative Examples 1 to 3

[0079] Example 2 ΔE Example 3 0.96 Example 4 0.99 Example 5 1.16 Example 6 1.29 Comparative Example 1 4.2 Comparative Example 2 3.16 Comparative Example 3 3.64

[0080] It can be seen from the data in Table 1 that the heat resistance of the iron oxide red composite pigment prepared in Examples 2 to 6 of the present invention is significantly higher than that of Comparative Example 1 (commercially available iron oxide red pigment), indicating that the present invention makes the crystal structure of the pigment more regular by doping other metal ions and controlling parameters such as reaction time, temperature and pressure, thereby improving the heat resistance of the pigment. By comparing Examples 2 to 6 with Comparative Example 3, it is found that the content of manganese dioxide added in Examples 2 and 3 is the highest, and the heat resistance of the final product is also the best, indicating that within a certain range of Mn 2+ The more the content introduced, the more significantly the heat resistance of the iron oxide pigment can be improved. By comparing Examples 2 to 6 with Comparative Example 2, it is found that when the content of the doped metal ions is low (not reaching the range specified by the present invention), although the heat resistance is improved compared to the commercially available iron oxide red pigment, it obviously does not reach the standard of the iron oxide red composite pigment obtained by the present invention, indicating that the present invention doped a specific proportion of metal ions such as manganese, cobalt, vanadium, copper and zinc in the original iron oxide pigment component and added related additives such as fillers, which can improve the thermal stability and heat resistance of the iron oxide pigment by forming a solid solution of iron oxide, especially Mn 2+ and Cu 2+ The introduction of can significantly improve the heat resistance of iron oxide pigments.

[0081] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a composite pigment of iron oxide modified by doping metal ions, characterized in that: The following steps are involved: Step 1, weighing 3 to 5 parts of calcined diatomaceous earth, 2 to 3 parts of calcined kaolin, 1 to 2 parts of mica powder, 15 to 25 parts of zinc oxide, 5 to 12 parts of manganese dioxide, 3 to 8 parts of cobalt oxide, 5 to 9 parts of vanadium pentoxide, 8 to 15 parts of copper oxide and 55 to 85 parts of iron oxide in a container, and stirring and mixing; Step 2, adding water, a dispersant and a binder into a container, heating and stirring to prepare a mixed slurry; Step 3, grinding the mixed slurry obtained in step 2, adding a filler and a consistency regulator, and letting it stand; Step 4, filtering, drying, powdering and sieving the mixed material after standing in step 3 to obtain a metal ion-doped modified iron oxide composite pigment.

2. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In the step 1, the components weighed in parts by weight are: 3 parts of calcined diatomaceous earth, 2 parts of calcined kaolin, 1 part of mica powder, 15 parts of zinc oxide, 12 parts of manganese dioxide, 3 parts of cobalt oxide, 9 parts of vanadium pentoxide, 12 parts of copper oxide and 85 parts of iron oxide.

3. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In the step 2, the added amounts of water, dispersant and binder are 100-200%, 0.1-0.3% and 2.0-3.0% of the total mass of the mixed material respectively.

4. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 3, characterized in that: In step 2, the added amounts of water, dispersant and binder are 180%, 0.3% and 2.0% of the total mass of the mixed material respectively.

5. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In the step 2, the dispersant is selected from one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate; and the binder is sodium silicate.

6. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In the step 2, the temperature for heating and stirring is 65-80°C.

7. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In step 3, the added amounts of the filler and consistency regulator are 0.5-0.8% and 0.3-0.5% of the total weight of the mixed material, respectively.

8. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: The filler is sodium metasilicate; the consistency regulator is polyethylene glycol.

9. The method for preparing the metal ion-doped modified iron oxide composite pigment according to claim 1, characterized in that: In step 4, the drying is carried out by oven drying until the moisture content does not exceed 0.5%.

10. The metal ion-doped modified iron oxide composite pigment prepared according to the method of any one of claims 1 to 9.