Metal net supported monolithic catalyst as well as preparation method and application thereof
The preparation of metal integral catalysts is simplified by electrochemical preparation methods, and the excellent performance of metal mesh such as copper mesh is used to solve the problems of cumbersome preparation process and high cost in the existing technology, achieving efficient catalytic oxidation CO performance and long-term stability , providing new industrial catalyst solutions.
Patent Information
- Application Number
- CN202410972287.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
AI Technical Summary
The preparation process of existing metal integral catalysts is cumbersome, time-consuming and labor-intensive, and the binding force between active species and metal support is low, which increases the preparation cost. The traditional wet chemistry method has little significance for process optimization.
The electrochemical preparation method is adopted to prepare a metal mesh-loaded integral catalyst through ultrasonic treatment, heat treatment and electrochemical redox pulse treatment. The excellent thermal conductivity and mechanical properties of metal mesh such as copper mesh are used to improve the catalyst's catalytic oxidation CO capability and stability.
The catalyst preparation process is simplified, the preparation efficiency and cost-effectiveness are improved, and the excellent catalytic oxidation CO performance and long-term stability are achieved, with good industrial application prospects.
Smart Images

Figure CN119034736A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation, and in particular to a metal mesh-supported integral catalyst and a preparation method and application thereof. Background Art
[0002] Carbon monoxide (CO) is a colorless, odorless and toxic gas. When the CO content in the air exceeds 0.1%, it may cause human poisoning. CO is mainly produced by incomplete combustion of fossil fuels and automobile exhaust emissions. With the widespread application of three-phase catalysts, the CO emissions from diesel vehicle exhaust have been greatly reduced. However, as one of the main sources of CO in industrial production, the steel industry has not received corresponding attention. With the improvement of national environmental protection requirements, there is also a considerable demand for the elimination of CO.
[0003] In industry, flue gas pollutants are mainly eliminated through monolithic catalysts. Since their first large-scale application in the 1970s, monolithic catalysts have played a vital role in the fields of chemical industry, environment, energy, etc. According to the different materials constituting the carrier, the carrier is generally divided into ceramic carrier and metal honeycomb carrier, which correspond to ceramic-based monolithic catalysts and metal-based monolithic catalysts. At present, although the preparation process of monolithic catalysts is relatively mature, its preparation process is still very cumbersome, time-consuming and labor-intensive.
[0004] Compared with ceramic carriers, the excellent thermal conductivity and mechanical properties of metal carriers give them inherent advantages when used in thermal catalysis. At present, the loading of active species on metal carriers still relies heavily on coating technology, and the low binding force between active species and metal carriers has always been a key factor restricting metal monolithic catalysts. In addition, metal carriers need to undergo additional treatment modifications to increase the specific surface area of the material, which will increase the preparation cost of the catalyst. Although a series of new methods for preparing metal-supported catalysts have emerged in recent years, such as Chinese patent CN 112742417A and Chinese patent CN 109999797 A, they are still concentrated on traditional wet chemical methods, which are of little significance for the optimization and improvement of the preparation process of metal-based monolithic catalysts. Summary of the invention
[0005] The purpose of the present invention is to provide a mild and simple electrochemical preparation method to overcome the defects of the above-mentioned prior art, and successfully prepare a new copper mesh supported monolithic catalyst. Thanks to the excellent thermal conductivity of the copper mesh, the prepared copper mesh catalyst shows excellent catalytic oxidation CO performance, has good thermal catalytic prospects, and provides a new idea for the preparation of industrial monolithic catalysts.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first aspect of the present invention provides a method for preparing a metal mesh-supported monolithic catalyst, comprising the following steps:
[0008] S1: The metal mesh is placed in anhydrous ethanol and deionized water for ultrasonic treatment and then dried to obtain a clean metal mesh;
[0009] S2: inserting the two cleaned metal meshes face to face into an electrolytic reaction cell, using a three-electrode system or a two-electrode system, wherein the two metal meshes serve as anode and cathode, adding an electrolyte, setting the electrochemical parameters, and performing electrochemical treatment using a chronopotentiometry at room temperature. After the treatment is completed, the metal meshes are taken out, ultrasonically cleaned in deionized water, and dried to obtain a metal mesh catalyst precursor;
[0010] S3: heat-treating the metal mesh precursor to obtain metal mesh catalyst I;
[0011] S4: placing the metal mesh catalyst I in deionized water for ultrasonic treatment and drying to obtain the metal mesh catalyst II;
[0012] S5: The metal mesh catalyst II is further heat-treated to obtain the metal mesh catalyst III, that is, the metal mesh-supported monolithic catalyst.
[0013] Furthermore, the metal mesh is one of a copper wire mesh, an iron mesh, and a nickel mesh.
[0014] Furthermore, the mesh size of the metal mesh is 20-400 meshes.
[0015] Furthermore, the electrolyte is selected from one of aqueous solutions of sodium sulfate, sodium chloride, sodium phosphate, potassium nitrate, potassium sulfate, potassium chloride, and potassium phosphate.
[0016] Furthermore, in the three-electrode system, saturated Ag / AgCl is used as a reference electrode.
[0017] Furthermore, in S2, the concentration range of the electrolyte aqueous solution is 0.001M-1M.
[0018] Furthermore, in S3, the gas composition of the heat treatment is pure inert gas, or oxygen + inert gas, and the treatment temperature is 180-400°C.
[0019] Furthermore, in S4, the ultrasonic time of the metal mesh catalyst I is 3-60 minutes.
[0020] The second aspect of the present invention provides a metal mesh-supported monolithic catalyst obtained by the above-mentioned preparation method.
[0021] A third aspect of the present invention provides a use of the metal mesh-supported monolithic catalyst in catalytic oxidation of CO.
[0022] Compared with the prior art, the present invention has the following technical advantages.
[0023] 1) The preparation method disclosed in the present invention has simple process, easy operation and mild conditions. Compared with the preparation method of the traditional monolithic catalyst, the preparation process is greatly simplified and the preparation efficiency is high.
[0024] 2) The metal mesh has excellent thermal conductivity, which makes the temperature distribution of the metal mesh monolithic catalyst very uniform during the thermal catalytic reaction. The good mechanical properties of the metal mesh make the metal mesh catalyst easy to process and highly adaptable to the reaction device.
[0025] 3) The metal mesh catalyst prepared in the present invention is prepared by an electrochemical method,
[0026] 4) It has excellent catalytic oxidation ability of CO and long-term catalyst stability, and has good prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a diagram showing the actual operation of preparing the copper mesh catalyst in the present invention;
[0028] Figure 2 This is a cross-sectional SEM image of the copper mesh catalyst of the present invention;
[0029] Figure 3 is the XRD diagram of the copper mesh catalyst in the present invention;
[0030] Figure 4 It is a data diagram of CO catalytic oxidation activity of each catalyst sample in the present invention;
[0031] Figure 5 This is a long-term CO catalytic oxidation stability diagram of the copper mesh catalyst sample in the present invention. DETAILED DESCRIPTION
[0032] On the whole, the present invention adopts the steps of electrochemical redox pulse treatment, heat treatment, and ultrasonic treatment to prepare a new type of supported integral catalyst with a metal mesh as the substrate. The method of the present invention gives the inert copper mesh excellent carbon monoxide oxidation ability and long-term catalytic stability, and has good thermal catalytic potential. Compared with the traditional wet chemical preparation method, this method greatly simplifies the preparation process, improves the preparation efficiency, saves manufacturing costs, and is easy to industrialize. The integral mesh catalyst is easy to put into use, and is easy to separate and recover. No additional separation operation is required, thereby saving operating costs, and has great research and application prospects.
[0033] In specific implementation, the preparation method of the metal mesh supported monolithic catalyst comprises the following steps:
[0034] Step 1: Place the cut 6×6 cm metal mesh in anhydrous ethanol and deionized water for ultrasonic treatment and dry to obtain a clean metal mesh;
[0035] Step 2: Insert the two cleaned metal meshes face to face into the customized electrolytic reaction cell, using a three-electrode system, in which the two metal meshes are the anode and cathode, saturated Ag / AgCl is the reference electrode, and a certain concentration of electrolyte is added to infiltrate the metal mesh (the infiltration area of the metal mesh is 24cm -2 ). After setting the electrochemical parameters, the electrochemical treatment was performed using the chronopotentiometry at room temperature. After the treatment was completed, the metal mesh was taken out, ultrasonically cleaned in deionized water, and dried to obtain a metal mesh catalyst precursor;
[0036] Step 3: heat-treating the metal mesh precursor to obtain metal mesh catalyst I;
[0037] Step 4: placing the metal mesh catalyst I in deionized water for ultrasonic treatment and drying to obtain the metal mesh catalyst II;
[0038] Step 5: The metal mesh catalyst II is further heat treated to obtain the metal mesh catalyst III.
[0039] During specific implementation, the metal mesh used is a copper mesh, an iron mesh, or a nickel mesh, preferably a copper mesh.
[0040] During specific implementation, the mesh size of the copper mesh used is 20-400 meshes, preferably 200 meshes.
[0041] During specific implementation, the electrode system used is a three-electrode system or a two-electrode system, preferably a three-electrode system.
[0042] During specific implementation, the electrolyte used is sodium nitrate, sodium sulfate, sodium chloride, sodium phosphate, potassium nitrate, potassium sulfate, potassium chloride, potassium phosphate solution, preferably sodium nitrate solution.
[0043] In specific implementation, the concentration range of the electrolyte used is 0.001M-1M, preferably 0.01M.
[0044] In the specific implementation, the electrochemical parameters involved include: (current value: 50-1500mA; corresponding current density: 2-60mA / cm 2 ; Single treatment time: 5-100s; Total treatment times: 50-800), preferably (current value: 180mA; corresponding current density: 7.5mA / cm 2 ; Single processing time: 40s; Total processing times: 300).
[0045] In specific implementation, the heat treatment temperature used is 180-400°C, preferably 200-300°C, and more preferably 210°C.
[0046] In specific implementation, the ultrasonic time of the metal mesh catalyst I is 3-60 minutes, preferably 15 minutes.
[0047] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.
[0048] Example 1
[0049] The synthesis of this embodiment comprises the following steps:
[0050] The cut copper mesh of 6×6 cm was placed in anhydrous ethanol and deionized water for ultrasonic treatment and dried to obtain a clean copper mesh;
[0051] The two cleaned copper meshes were inserted face to face into a custom-made electrolytic reaction cell. A three-electrode system was used, in which the two copper meshes were the anode and cathode, and saturated Ag / AgCl was used as the reference electrode. 0.01 M sodium nitrate electrolyte was added to infiltrate the copper meshes (the infiltration area of the copper mesh was 24 cm 2 ). Set the current value: 180mA; the corresponding current density: 7.5mA / cm 2 ; Single treatment time: 40s; Total treatment times: 300. Electrochemical treatment was performed using chronopotentiometry at room temperature. After the treatment, the copper mesh was taken out, ultrasonically cleaned in deionized water for 5 minutes, and dried to obtain a copper mesh monolithic catalyst precursor;
[0052] The copper mesh catalyst precursor was heat treated at 210° C. in an argon atmosphere for 1 h to obtain copper mesh catalyst I.
[0053] Example 2
[0054] The copper mesh catalyst I prepared in Example 1 was placed in deionized water for ultrasonic treatment for 15 minutes and dried to obtain the copper mesh catalyst II.
[0055] Example 3
[0056] The copper mesh catalyst II prepared in Example 2 was heat treated at 210° C. in a 20% O 2 / Ar atmosphere for 1 h to obtain the copper mesh catalyst III.
[0057] Comparative Example 1
[0058] The cut copper mesh of 6×6 cm was placed in anhydrous ethanol and deionized water for ultrasonic treatment and dried to obtain a clean untreated copper mesh.
[0059] Comparative Examples 2-5
[0060] The preparation process of Comparative Examples 2-5 is the same, only the CuO loading is different, and the synthesis steps include: 4g of silica carrier is ultrasonically dispersed in deionized water to form a slurry, and then a certain amount of copper nitrate solution is added and mechanically stirred for 1 hour. Then, an excess of 2M sodium carbonate solution is added dropwise to adjust the pH to 10, and stirring is continued for 90 minutes. After the end, the precipitate is collected by centrifugation washing with deionized water, dried at 80°C overnight, and calcined at 450°C for 3 hours to obtain a 15-45% CuO / SiO2 catalyst. The CuO loading in the embodiment is included in the loading range of the comparative example.
[0061] Verification Example 1
[0062] The CO catalytic oxidation activity of Examples 1-3 and Comparative Examples 1-5 was evaluated in turn. Specifically, the copper mesh catalyst was cut into small discs with a diameter of 4 mm, and the CuO / SiO2 catalyst was sieved into particles of 60-80 mesh and then loaded into a quartz reaction tube, and the evaluation was carried out in a microreactor. The gas volume composition was 1% CO, 20% O2 and 80% Ar, and the gas flow rate was 50 mL min -1 , the reaction space velocity is 60000mL g cat -1 h -1 The activity evaluation temperature range is 80-120℃.
[0063] Figure 1 This is a diagram of the actual operation of preparing the catalyst in the present invention.
[0064] Figure 2 The cross-sectional SEM image of the copper mesh catalyst in the present invention. Figure 1 It can be seen that the copper mesh catalyst I after electrochemical treatment has a three-layer structure, and the copper mesh catalyst II after ultrasonic treatment has only a two-layer structure. This shows that the prepared catalyst intermediate layer has good mechanical stability.
[0065] Figure 3 The XRD pattern of the copper mesh catalyst in the present invention shows that the copper mesh catalyst has a Cu / Cu2O / CuO structure. The ultrasonic treatment of the copper mesh catalyst II only leads to a decrease in the XRD characteristic peak intensity of CuO, indicating that Figure 2 The outer layer that falls off is CuO.
[0066] Figure 4 The CO catalytic oxidation activity data of each catalyst sample in the present invention are shown in FIG. Figure 2It can be seen that the electrochemically treated copper mesh catalyst has excellent CO oxidation ability. Although the activity of copper mesh catalyst II decreased compared with copper mesh catalyst I after ultrasonic treatment, the activity of copper mesh catalyst III returned to its original level after another heat treatment. In contrast, the untreated copper mesh is completely inactive. In addition, the CuO / SiO2 comparison is basically inactive in the same temperature range. It can be concluded that based on the normalization of the mass of the active components, the copper mesh catalyst prepared by the electrochemical in-situ preparation method exhibits ultra-high low-temperature catalytic activity in the catalytic oxidation reaction, with unexpected technical effects, proving that our electrochemically prepared copper mesh catalyst has great superiority.
[0067] Figure 5 This is a graph showing the long-term catalytic oxidation stability of CO by the copper mesh catalyst sample III of the present invention. Figure 3 It can be found that after a long-term test of 100 hours, the prepared copper mesh catalyst can still maintain an activity of about 90%, proving that it has good catalyst stability.
[0068] The above embodiment provides a simple method for synthesizing a metal monolithic catalyst, which has high preparation efficiency, greatly simplified preparation process and low cost compared with the traditional wet chemical method. The method gives the inert metal mesh excellent CO catalytic oxidation ability and has good thermal catalytic potential. The method proposes a new idea for the preparation process of the existing metal monolithic catalyst and has good application prospects.
[0069] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a metal mesh supported monolithic catalyst, characterized in that: The following steps are involved: S1: The metal mesh is placed in anhydrous ethanol and deionized water for ultrasonic treatment and then dried to obtain a clean metal mesh; S2: inserting the two cleaned metal meshes face to face into an electrolytic reaction cell, using a three-electrode system or a two-electrode system, wherein the two metal meshes serve as anode and cathode, adding an electrolyte, setting the electrochemical parameters, and performing electrochemical treatment using a chronopotentiometry at room temperature. After the treatment is completed, the metal meshes are taken out, ultrasonically cleaned in deionized water, and dried to obtain a metal mesh catalyst precursor; S3: heat-treating the metal mesh precursor to obtain metal mesh catalyst I; S4: placing the metal mesh catalyst I in deionized water for ultrasonic treatment and drying to obtain the metal mesh catalyst II; S5: The metal mesh catalyst II is further heat-treated to obtain the metal mesh catalyst III, that is, the metal mesh-supported monolithic catalyst.
2. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: The metal mesh is one of a copper wire mesh, an iron mesh and a nickel mesh.
3. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: The mesh number of the metal mesh is 20-400 meshes.
4. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: The electrolyte is selected from one of aqueous solutions of sodium sulfate, sodium chloride, sodium phosphate, potassium nitrate, potassium sulfate, potassium chloride, and potassium phosphate.
5. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: In the three-electrode system, saturated Ag / AgCl is the reference electrode.
6. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: In S2, the concentration range of the electrolyte aqueous solution is 0.001M-1M.
7. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: In S3, the gas composition of the heat treatment is pure inert gas, or oxygen + inert gas, and the treatment temperature is 180-400°C.
8. The method for preparing a metal mesh supported monolithic catalyst according to claim 1, characterized in that: In S4, the ultrasonic time of the metal mesh catalyst I is 3-60 minutes.
9. A metal mesh-supported monolithic catalyst obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the metal mesh-supported monolithic catalyst as claimed in claim 9 in catalytic oxidation of CO.