Coal-based powdered activated carbon with high strength and high specific surface area and preparation method of coal-based powdered activated carbon

By mixing anthracite, lignite and weak viscous coal in a specific proportion and grinding and heat treatment, combining phosphoric acid and zinc chloride and other treatment steps, the pore structure of activated carbon is optimized, and the problem of insufficient mechanical strength and specific surface area of ​​activated carbon in coal-based powder is solved. It achieves efficient adsorption and durability improvement.

CN119038545AActive Publication Date: 2024-11-29山东韩研活性炭有限公司

Patent Information

Application Number
CN202411200895.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing coal-based powder activated carbon has shortcomings in terms of mechanical strength and specific surface area, which is difficult to meet the requirements of efficient adsorption and durability.

Method used

By mixing anthracite, lignite and weak viscous coal in a specific proportion and grinding and heat treatment, combining phosphoric acid, zinc chloride, oxalic acid and other treatment steps, the pore structure and chemical stability of activated carbon are optimized to form a high-strength, high specific surface area coal quality with high strength and high specific surface area Powder activated carbon.

Benefits of technology

It significantly improves the adsorption capacity and mechanical strength of activated carbon, enhances the adsorption capacity of organic matter and heavy metal ions, and improves its stability and durability under various conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to coal-based powdered activated carbon with high strength and high specific surface area and a preparation method thereof, and belongs to the technical field of activated carbon preparation. By mixing anthracite, lignite and weakly caking coal and carrying out grinding and heat treatment, the prepared activated carbon has more types of pore structures, so that the specific surface area is increased, the adsorption capacity of the activated carbon is improved, and subsequent steps of phosphoric acid treatment, zinc chloride addition, ultrasonic treatment and the like are beneficial to further optimization of the pore structures and increase of the specific surface area; according to the formula, the final product has higher specific surface area and porosity, the mechanical strength of the activated carbon can be improved by adding the coal pitch and the aluminum oxide, the activated carbon is more durable in the using process, chemical components in the coal pitch can promote formation and expansion of pores in the carbonization process, and therefore the pore structure of the activated carbon is optimized, and the service life of the activated carbon is prolonged. The added aluminum oxide can be combined with the surface of the activated carbon through chemical or physical action to form a layer of stable protective film or modified layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of activated carbon preparation, and relates to a coal-based powdered activated carbon with high strength and high specific surface area and a preparation method thereof. Background Art

[0002] The main raw material of coal-based powdered activated carbon is coal, especially high-quality anthracite. This type of coal has low ash content and high fixed carbon content, making it an ideal raw material for preparing high-quality activated carbon.

[0003] Coal-based granular activated carbon has high strength, developed pores, large specific surface area, and especially large micropore volume, which is unique. Coal-based activated carbon has a strong adsorption capacity for organic matter in various waters, free chlorine, and harmful gases in the air. It is an excellent adsorbent for deep purification of urban drinking water, and is used to remove bacteria and toxic gases in the air. Coal-based activated carbon has a developed pore structure, good chemical stability and mechanical strength, and is an excellent broad-spectrum carbonaceous adsorption material. Coal-based activated carbon can be mainly divided into coal-based granular activated carbon and coal-based powdered activated carbon. According to different uses, it can be divided into activated carbon for water purification, air purification, decolorization, solvent recovery, injection, protection and other purposes. Because it is acid-resistant, alkali-resistant, and heat-resistant, it can be easily regenerated. Therefore, activated carbon is an indispensable carbonaceous adsorption material in industrial production and environmental protection in modern society. Summary of the invention

[0004] The object of the present invention is to provide a high-strength and high-specific-surface-area coal-based powdered activated carbon and a preparation method thereof, which has the characteristics of wear resistance and high specific-surface-area.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-strength and high-specific-surface-area coal-based powdered activated carbon, wherein the activated carbon raw materials are as follows: by mass percentage, 75-85% of modified coal powder, 3-5% of coal tar pitch, 3-5% of aluminum oxide, 3-5% of dispersant, and 5-10% of deionized water.

[0007] Wherein, the preparation method of the modified coal powder is:

[0008] S1: anthracite, lignite and weakly caking coal are mixed in a mass ratio of (2-5):2:1, ground in a ball mill at a speed of 500 r / min for 4-6 h, and sieved to obtain a mixture A;

[0009] S2: Spread the mixture A evenly to a thickness of 3 to 5 cm, first introduce water vapor for heat treatment for 0.5 to 2 h at a heat treatment temperature of 800 to 950° C., then introduce carbon dioxide for purging, slowly raise the temperature to 120° C. while purging, and continue purging at 120° C. for 6 h to obtain a mixture B;

[0010] S3: Disperse the mixture B in a phosphoric acid solution with a mass fraction of 10% to obtain a solid-liquid mixture C with a mass fraction of 30-50%, stir at a speed of 200 r / min, and dropwise add a zinc chloride solution with a mass fraction of 20% while stirring. The stirring time is 2 hours, wherein the volume ratio of the solid-liquid mixture C to the zinc chloride solution is 2:1. After the stirring is completed, ultrasonicate for 0.5 hours, filter, and dry at 110°C for 8 hours to obtain a mixture D;

[0011] S4: In an oxygen-free environment, the mixture D is subjected to a carbonization reaction at a carbonization temperature of 550 to 650° C. for a carbonization time of 4 to 5 hours. After the carbonization is completed, the mixture is cooled to room temperature to obtain a carbonized product E;

[0012] S5: Add 2-3wt% oxalic acid and 0.5-1wt% zinc chloride to the carbonized product E, grind at a rotation speed of 500r / min for 1h, dry the ground mixture at 110°C for 8h, transfer it to a nitrogen atmosphere after drying, and roast it in a muffle furnace at 400°C for 2h. After roasting, cool it to room temperature, grind it to a particle size of 300 mesh, and obtain the modified coal powder.

[0013] Furthermore, the dispersant is polyethylene glycol, and the number average molecular weight is 20,000 to 25,000.

[0014] Furthermore, the ash content of the anthracite, lignite and slightly caking coal in S1 is 20-25wt%.

[0015] Furthermore, the particle size of the mixture A in S1 is 200 mesh.

[0016] Furthermore, the amount of water vapor introduced into S2 is 1.5 to 2 kg / h.

[0017] Furthermore, the flow rate of the carbon dioxide in S2 is 10 m / s.

[0018] Furthermore, the dropping rate of the zinc chloride solution in S3 is 5 seconds per drop.

[0019] Furthermore, the heating rate of the muffle furnace in S5 is 5°C / min.

[0020] A method for preparing high-strength and high-specific-surface-area coal-based powdered activated carbon, the specific process of the method for preparing high-strength and high-specific-surface-area coal-based powdered activated carbon is as follows:

[0021] S91: uniformly mix the modified coal powder, coal tar pitch and alumina according to the formula ratio, and grind at a speed of 500-600 r / min for 4 hours to obtain a mixture F;

[0022] S92: Disperse the mixture F in deionized water, add a dispersant, perform ultrasonication for 2 h, filter, freeze in liquid nitrogen for 15 to 20 min, and dry at -70 to -50°C under vacuum for 10 to 12 h to obtain a mixture G;

[0023] S93: Grind the mixture G to obtain the coal-based powdered activated carbon.

[0024] Furthermore, the particle size of the coal-based powdered activated carbon prepared in S93 is 500 mesh.

[0025] By mixing different types of coal (anthracite, lignite, weakly sticky coal) and grinding and heat treating them, the activated carbon produced has more types of pore structures, thereby increasing the specific surface area and improving its adsorption capacity. Subsequent steps such as phosphoric acid treatment, zinc chloride addition and ultrasonic treatment help to further optimize the pore structure and increase the specific surface area.

[0026] During the preparation process, multiple heat treatments, carbonization and calcination under nitrogen atmosphere are used to improve the chemical stability of activated carbon, so that it can maintain stable mechanical strength under various conditions. Long-term grinding and heat treatment will make the activated carbon particles more tightly bonded, thereby improving its compression and wear resistance, which is crucial for the long-term stability and durability of activated carbon in practical applications.

[0027] Anthracite has good hardness and high chemical stability. It is suitable for direct crushing or grinding and then forming into granular carbon. The activated carbon made from it has well-developed micropores, large micropore volume, large specific surface area, and good adsorption performance for vapor and gas. Lignite resources are abundant, low in price, have more pores, and rich functional groups. It has especially good adsorption, complexation and exchange properties. Its carbonization process directly forms a solid state without generating liquid, which is beneficial to maintaining the structure of activated carbon. Weakly sticky coal is between anthracite and lignite. It has both a certain hardness and a certain pore structure. It is suitable for mixing with other types of coal to adjust the performance of the final product.

[0028] The high hardness and high adsorption performance of anthracite can be combined with the rich pores and functional groups of lignite, while weakly sticky coal can play a bridging role in making the mixed raw materials more uniform and stable. During the pyrolysis and activation process, the coal quality structure of different types of coal will change, forming different pore structures. The synergistic effect of these pores can optimize the pore structure of activated carbon, so that it has sufficient micropores to provide high specific surface area and excellent adsorption performance, and contains an appropriate amount of mesopores and macropores to improve mass transfer efficiency and adsorption kinetics; during the pyrolysis and activation process, cross-linking, cracking, and polycondensation reactions will occur between different types of coal in the mixed raw materials. These reactions can promote the formation of activated carbon and the development of pore structure. The functional groups in lignite can react with the carbon skeleton in anthracite to form more stable chemical bonds and more complex pore structures. At the same time, weakly sticky coal can also act as a catalyst or reaction intermediate to promote these chemical reactions.

[0029] Steam heat treatment can improve the bonding index of coal and optimize the pyrolysis performance of coal; steam treatment can promote the decomposition of oxygen-containing functional groups in coal, reduce hydrogen consumption in the process of coal utilization, and thus improve the calorific value of coal; the hydrogen in the steam can be added to the coal through the hydrolysis of oxygen-containing functional groups under the synergistic effect of free radical and ion effects, effectively supplying hydrogen to stabilize medium molecular weight free radical fragments; appropriate steam heat treatment can also help reduce pollutants produced by coal during combustion or gasification, such as sulfur oxides and nitrogen oxides.

[0030] Steam thermal treatment heats the coal powder and introduces steam, causing the organic matter in the coal to react chemically with the steam at high temperature. These reactions include pyrolysis, hydrolysis, and oxidation-reduction, which can change the chemical structure and physical properties of the coal. Specifically, water vapor can penetrate into the pores of the coal and react with the carbon, hydrogen, oxygen and other elements in the coal to generate CO, CO 2 , H 2 Gaseous products and solid residues. These reactions can break the chemical bonds in the coal and form new pore structures, thereby improving the adsorption, reactivity and utilization of the coal.

[0031] Carbon dioxide treatment can improve the microstructure of coal, making it easier to react with gasification agents or combustion agents, thereby increasing the conversion rate and utilization rate of coal; compared with traditional coal treatment methods, the carbon dioxide treatment process has low energy consumption and does not produce secondary pollution.

[0032] Phosphorylation heat treatment introduces phosphates to react chemically with the surface of coal powder to form a phosphate layer, which can significantly enhance the wear resistance, corrosion resistance and oxidation resistance of coal powder. This is of great significance for improving the stability and durability of coal powder during subsequent processing and use. Phosphoric acid also plays a skeleton role during the heat treatment process, accompanied by the formation of micropores. This helps to optimize the pore structure of coal powder and improve its adsorption performance and reaction activity. The ionization and dehydration of phosphoric acid can promote the elimination of hydroxyl groups in coal powder and the expansion of cross-linked structures, which is conducive to the subsequent chemical reactions.

[0033] Zinc chloride as a catalyst can accelerate the cracking and conversion process of coal powder at high temperature, thereby changing the chemical composition and physical properties of coal powder; zinc chloride can react with sulfides in coal to precipitate and separate them from coal powder. This helps to reduce the emission of sulfur oxide pollutants generated during the combustion or gasification of coal powder; through the treatment of zinc chloride, the combustible components in coal powder can be more easily extracted and utilized, thereby improving the utilization rate of coal powder.

[0034] The role of zinc chloride in the thermal treatment of pulverized coal is mainly based on its catalytic properties and its ability to react with substances in coal. At high temperatures, zinc chloride can penetrate into the pores of pulverized coal and react with organic and inorganic matter in it. These reactions may include cracking, oxidation, reduction and other processes, resulting in changes in the chemical composition and physical properties of the pulverized coal. In particular, the reaction of zinc chloride with sulfides in coal can significantly reduce the sulfur content in pulverized coal and reduce the pollution caused by its combustion.

[0035] Through the carbonization reaction, the volatile matter and other combustible components in the coal powder are further removed, thereby increasing the carbon content of the coal powder, which helps to improve the combustion performance and calorific value of the coal powder. During the carbonization process, the structure of the coal powder will change, the porosity will increase, and the surface area will increase. These changes are conducive to improving the adsorption capacity and reaction activity of the coal powder. At high temperatures, the organic matter in the coal powder undergoes pyrolysis reaction to generate CO, CO 2 , H 2 Gas and coke, these gases are gradually released as the temperature rises, leaving solid products mainly composed of carbon. As the volatile matter is removed, the pore structure of the coal powder changes and the porosity increases, which helps the coal powder to better react or adsorb with other substances in subsequent applications.

[0036] Oxalic acid can remove metal ions and other impurities in coal powder and improve the purity of coal powder. Zinc chloride, as a catalyst and auxiliary agent, can promote the dispersion of coal powder particles and prevent them from agglomerating in subsequent applications. At the same time, the addition of zinc chloride can continue to participate in the chemical reaction on the surface of coal powder to form a stable protective layer. After roasting, carbon-oxygen bonds, carbon-chlorine bonds, etc. are formed on the surface of coal powder. The formation of these chemical bonds helps to change the surface properties and catalytic performance of coal powder, form sites with catalytic activity, and improve the catalytic performance of coal powder in the reaction.

[0037] The formula of the present invention combines a variety of ingredients that are beneficial to the adsorption performance of activated carbon, so that the final product has a higher specific surface area and porosity, thereby enhancing the adsorption capacity of pollutants such as organic matter and heavy metal ions. The addition of coal tar and aluminum oxide helps to improve the mechanical strength of activated carbon, making it more durable during use. The chemical components in coal tar promote the formation and expansion of pores during the carbonization process, thereby optimizing the pore structure of activated carbon. The addition of aluminum oxide can be combined with the surface of activated carbon through chemical or physical effects to form a stable protective film or modified layer, which can enhance its acid and alkali resistance and antioxidant properties; the addition of a dispersant helps to improve the dispersibility of activated carbon particles in the solution, making it easier to handle and operate in practical applications.

[0038] Beneficial effects of the present invention:

[0039] (1) The present invention mixes anthracite, lignite and weakly sticky coal and grinds and heat treats them, so that the prepared activated carbon has more types of pore structures, thereby increasing the specific surface area and improving its adsorption capacity. Subsequent steps such as phosphoric acid treatment, zinc chloride addition and ultrasonic treatment are helpful to further optimize the pore structure and increase the specific surface area.

[0040] (2) The formula of the present invention combines a variety of ingredients that are beneficial to the adsorption performance of activated carbon, so that the final product has a higher specific surface area and porosity, thereby enhancing the adsorption capacity of pollutants such as organic matter and heavy metal ions. The addition of coal tar and alumina helps to improve the mechanical strength of activated carbon, making it more durable during use. The chemical components in coal tar promote the formation and expansion of pores during the carbonization process, thereby optimizing the pore structure of activated carbon. The addition of alumina can combine with the surface of activated carbon through chemical or physical effects to form a stable protective film or modified layer, which can enhance its acid and alkali resistance and antioxidant properties. The addition of dispersant helps to improve the dispersibility of activated carbon particles in solution, making it easier to handle and operate in practical applications. DETAILED DESCRIPTION

[0041] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.

[0042] Example 1

[0043] Modified coal powder 80%, coal tar 5%, alumina 5%, polyethylene glycol-200005%, deionized water 5%,

[0044] Wherein, the preparation method of the modified coal powder is:

[0045] S1: anthracite, lignite and slightly caking coal are mixed in a mass ratio of 4:2:1, the ash content of anthracite, lignite and slightly caking coal is 20wt%, and the mixture is ground in a ball mill at a speed of 500r / min for 5h, and sieved to obtain a mixture A, the particle size of the mixture A is 200 mesh;

[0046] S2: Mixture A was evenly spread to a thickness of 3 cm, and water vapor was introduced for heat treatment at a rate of 2 kg / h, the treatment time was 1 h, and the heat treatment temperature was 900°C. Carbon dioxide was then introduced for purging at a flow rate of 10 m / s. The temperature was slowly raised to 120°C while purging, and the purging was continued at 120°C for 6 h to obtain mixture B;

[0047] S3: Disperse the mixture B in a phosphoric acid solution with a mass fraction of 10% to obtain a solid-liquid mixture C with a mass fraction of 40%, stir at a speed of 200 r / min, and dropwise add a zinc chloride solution with a mass fraction of 20% while stirring. The dropping rate of the zinc chloride solution is 5 seconds / drop, and the stirring time is 2 hours. The volume ratio of the solid-liquid mixture C to the zinc chloride solution is 2:1. After the stirring is completed, ultrasonicate for 0.5 hours, filter, and dry at 110°C for 8 hours to obtain a mixture D;

[0048] S4: In an oxygen-free environment, the mixture D is subjected to a carbonization reaction at a carbonization temperature of 600° C. for a carbonization time of 4 h. After the carbonization is completed, the mixture is cooled to room temperature to obtain a carbonized product E;

[0049] S5: Add 3wt% oxalic acid and 1wt% zinc chloride to the carbonized product E, grind at a speed of 500r / min for 1h, dry the ground mixture at 110°C for 8h, transfer it to a nitrogen atmosphere after drying, and roast it in a muffle furnace at 400°C for 2h with a heating rate of 5°C / min. After roasting, cool it to room temperature, grind it to a particle size of 300 mesh, and obtain the modified coal powder.

[0050] The specific process of the method for preparing coal-based powdered activated carbon is as follows:

[0051] S91: uniformly mix the modified coal powder, coal tar pitch and alumina according to the formula ratio, and grind at a speed of 500-600 r / min for 4 hours to obtain a mixture F;

[0052] S92: Disperse the mixture F in deionized water, add a dispersant, perform ultrasonication for 2 h, filter, freeze in liquid nitrogen for 20 min, and dry at -60°C under vacuum for 12 h to obtain a mixture G;

[0053] S93: Grind the mixture G to obtain the coal-based powdered activated carbon, wherein the particle size of the obtained coal-based powdered activated carbon is 500 meshes.

[0054] Example 2

[0055] Modified coal powder 85%, coal tar 3%, alumina 3%, polyethylene glycol-250003%, deionized water 6%,

[0056] Wherein, the preparation method of the modified coal powder is:

[0057] S1: anthracite, lignite and slightly caking coal are mixed in a mass ratio of 2:2:1, the ash content of anthracite, lignite and slightly caking coal is 25wt%, and the mixture is ground in a ball mill at a speed of 500r / min for 6h, and sieved to obtain a mixture A, the particle size of the mixture A is 200 mesh;

[0058] S2: Mixture A was evenly spread to a thickness of 3 cm, and water vapor was introduced for heat treatment at a rate of 1.5 kg / h, the treatment time was 0.5 h, and the heat treatment temperature was 800°C. Carbon dioxide was then introduced for purging at a flow rate of 10 m / s. The temperature was slowly raised to 120°C while purging, and the purging was continued at 120°C for 6 h to obtain mixture B;

[0059] S3: Disperse the mixture B in a phosphoric acid solution with a mass fraction of 10% to obtain a solid-liquid mixture C with a mass fraction of 50%, stir at a speed of 200 r / min, and while stirring, dropwise add a zinc chloride solution with a mass fraction of 20%, with a dropping rate of the zinc chloride solution of 5 seconds / drop, and stir for 2 hours, wherein the volume ratio of the solid-liquid mixture C to the zinc chloride solution is 2:1, and after stirring, ultrasonicate for 0.5 hours, filter, and dry at 110°C for 8 hours to obtain a mixture D;

[0060] S4: In an oxygen-free environment, the mixture D is subjected to a carbonization reaction at a carbonization temperature of 550° C. for a carbonization time of 4 to 5 hours. After the carbonization is completed, the mixture is cooled to room temperature to obtain a carbonized product E;

[0061] S5: Add 2wt% oxalic acid and 0.5wt% zinc chloride to the carbonized product E, grind at a speed of 500r / min for 1h, dry the ground mixture at 110°C for 8h, transfer it to a nitrogen atmosphere after drying, and roast it in a muffle furnace at 400°C for 2h with a heating rate of 5°C / min. After roasting, cool it to room temperature, grind it to a particle size of 300 mesh, and obtain the modified coal powder.

[0062] The specific process of the method for preparing coal-based powdered activated carbon is as follows:

[0063] S91: uniformly mix the modified coal powder, coal tar pitch and alumina according to the formula ratio, and grind at a speed of 500-600 r / min for 4 hours to obtain a mixture F;

[0064] S92: Disperse the mixture F in deionized water, add a dispersant, perform ultrasonication for 2 h, filter, freeze in liquid nitrogen for 15 min, and dry at -50°C under vacuum for 10 h to obtain a mixture G;

[0065] S93: Grind the mixture G to obtain the coal-based powdered activated carbon, wherein the particle size of the obtained coal-based powdered activated carbon is 500 meshes.

[0066] Example 3

[0067] Modified coal powder 75%, coal tar pitch 5%, alumina 5%, polyethylene glycol-200005%, deionized water 10%,

[0068] Wherein, the preparation method of the modified coal powder is:

[0069] S1: anthracite, lignite and slightly caking coal are mixed in a mass ratio of 5:2:1, the ash content of anthracite, lignite and slightly caking coal is 20wt%, and the mixture is ground in a ball mill at a speed of 500r / min for 6h, and sieved to obtain a mixture A, the particle size of the mixture A is 200 mesh;

[0070] S2: Mixture A was evenly spread with a thickness of 5 cm, and water vapor was first introduced for heat treatment at a rate of 2 kg / h for 2 h. The heat treatment temperature was 950°C, and then carbon dioxide was introduced for purging at a flow rate of 10 m / s. While purging, the temperature was slowly raised to 120°C, and purging was continued at 120°C for 6 h to obtain mixture B;

[0071] S3: Disperse the mixture B in a phosphoric acid solution with a mass fraction of 10% to obtain a solid-liquid mixture C with a mass fraction of 30%, stir at a speed of 200 r / min, and dropwise add a zinc chloride solution with a mass fraction of 20% while stirring. The dropping rate of the zinc chloride solution is 5 seconds / drop, and the stirring time is 2 hours. The volume ratio of the solid-liquid mixture C to the zinc chloride solution is 2:1. After the stirring is completed, ultrasonicate for 0.5 hours, filter, and dry at 110°C for 8 hours to obtain a mixture D;

[0072] S4: In an oxygen-free environment, the mixture D is subjected to a carbonization reaction at a carbonization temperature of 650° C. for a carbonization time of 4 h. After the carbonization is completed, the mixture is cooled to room temperature to obtain a carbonized product E;

[0073] S5: Add 3wt% oxalic acid and 1wt% zinc chloride to the carbonized product E, grind at a speed of 500r / min for 1h, dry the ground mixture at 110°C for 8h, transfer it to a nitrogen atmosphere after drying, and roast it in a muffle furnace at 400°C for 2h with a heating rate of 5°C / min. After roasting, cool it to room temperature, grind it to a particle size of 300 mesh, and obtain the modified coal powder.

[0074] The specific process of the method for preparing coal-based powdered activated carbon is as follows:

[0075] S91: uniformly mix the modified coal powder, coal tar pitch and alumina according to the formula ratio, and grind at a speed of 500-600 r / min for 4 hours to obtain a mixture F;

[0076] S92: Disperse the mixture F in deionized water, add a dispersant, perform ultrasonication for 2 h, filter, freeze in liquid nitrogen for 20 min, and dry at -70°C under vacuum for 12 h to obtain a mixture G;

[0077] S93: Grind the mixture G to obtain the coal-based powdered activated carbon, wherein the particle size of the obtained coal-based powdered activated carbon is 500 meshes.

[0078] Comparative Example 1

[0079] In this comparative example, only anthracite and weakly caking coal were used in the coal powder modification process, and the remaining steps were consistent with Example 1.

[0080] Comparative Example 2

[0081] In this comparative example, only lignite and weakly caking coal were used in the coal powder modification process, and the remaining steps were consistent with Example 1.

[0082] Comparative Example 3

[0083] In this comparative example, the water vapor heat treatment and carbon dioxide treatment in S2 are not performed during the coal powder modification process, and the remaining steps are consistent with Example 1.

[0084] Comparative Example 4

[0085] In this comparative example, phosphoric acid and zinc chloride treatment in S3 is not performed during the coal powder modification process, and the remaining steps are consistent with Example 1.

[0086] Comparative Example 5

[0087] In this comparative example, the oxalic acid and zinc chloride treatment in S5 is not performed during the coal powder modification process, and the remaining steps are consistent with Example 1.

[0088] Comparative Example 6

[0089] In this comparative example, coal tar was not added during the preparation process, and the remaining steps were consistent with those in Example 1.

[0090] Comparative Example 7

[0091] In this comparative example, no alumina was added during the preparation process, and the remaining steps were consistent with those in Example 1.

[0092] The performance tests of the embodiments and comparative examples were carried out, the mechanical strength tests were carried out according to the standard of GB / T7702.3-2008, and the specific surface area tests were carried out according to the standard of GB / T7702.20-2008. The test results are summarized in the following table:

[0093] Mechanical strength (%) <![CDATA[Specific surface area (m 2 / g)]]> Example 1 99 1305 Example 2 98 1281 Example 3 98 1287 Comparative Example 1 96 1002 Comparative Example 2 89 1129 Comparative Example 3 93 984 Comparative Example 4 91 1135 Comparative Example 5 91 1142 Comparative Example 6 94 990 Comparative Example 7 90 1192

[0094] Experiments show that modification of coal powder makes the activated carbon have better mechanical strength and specific surface area, adding coal tar into the formula makes the activated carbon have better specific surface area, and adding alumina improves the mechanical strength of the activated carbon.

[0095] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A high-strength and high-specific-surface-area coal-based powdered activated carbon, characterized in that: The activated carbon raw materials are as follows: by mass percentage, modified coal powder 75-85%, coal tar pitch 3-5%, aluminum oxide 3-5%, dispersant 3-5%, deionized water 5-10%, Wherein, the preparation method of the modified coal powder is: S1: anthracite, lignite and weakly caking coal are mixed in a mass ratio of (2-5):2:1, ground in a ball mill at a speed of 500 r / min for 4-6 h, and sieved to obtain a mixture A; S2: Spread the mixture A evenly to a thickness of 3 to 5 cm, first introduce water vapor for heat treatment for 0.5 to 2 h at a heat treatment temperature of 800 to 950° C., then introduce carbon dioxide for purging, slowly raise the temperature to 120° C. while purging, and continue purging at 120° C. for 6 h to obtain a mixture B; S3: Disperse the mixture B in a phosphoric acid solution with a mass fraction of 10% to obtain a solid-liquid mixture C with a mass fraction of 30-50%, stir at a speed of 200 r / min, and dropwise add a zinc chloride solution with a mass fraction of 20% while stirring. The stirring time is 2 hours, wherein the volume ratio of the solid-liquid mixture C to the zinc chloride solution is 2:

1. After the stirring is completed, ultrasonicate for 0.5 hours, filter, and dry at 110°C for 8 hours to obtain a mixture D; S4: In an oxygen-free environment, the mixture D is subjected to a carbonization reaction at a carbonization temperature of 550 to 650° C. for a carbonization time of 4 to 5 hours. After the carbonization is completed, the mixture is cooled to room temperature to obtain a carbonized product E; S5: Add 2-3wt% oxalic acid and 0.5-1wt% zinc chloride to the carbonized product E, grind at a rotation speed of 500r / min for 1h, dry the ground mixture at 110°C for 8h, transfer it to a nitrogen atmosphere after drying, and roast it in a muffle furnace at 400°C for 2h. After roasting, cool it to room temperature, grind it to a particle size of 300 mesh, and obtain the modified coal powder.

2. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The dispersant is polyethylene glycol, and the number average molecular weight is 20000-25000.

3. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The ash content of the anthracite, lignite and slightly caking coal in S1 is 20-25wt%.

4. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The particle size of the mixture A in S1 is 200 mesh.

5. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The amount of water vapor introduced into the S2 is 1.5-2 kg / h.

6. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The flow rate of carbon dioxide in S2 is 10m / s.

7. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The dropping rate of the zinc chloride solution in S3 is 5 seconds / drop.

8. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 1, characterized in that: The heating rate of the muffle furnace in S5 is 5°C / min.

9. A method for preparing a high-strength and high-specific-surface-area coal-based powdered activated carbon according to any one of claims 1 to 8, characterized in that: The specific process of the method for preparing coal-based powdered activated carbon is as follows: S91: uniformly mix the modified coal powder, coal tar pitch and alumina according to the formula ratio, and grind at a speed of 500-600 r / min for 4 hours to obtain a mixture F; S92: Disperse the mixture F in deionized water, add a dispersant, perform ultrasonication for 2 h, filter, freeze in liquid nitrogen for 15 to 20 min, and dry at -70 to -50°C under vacuum for 10 to 12 h to obtain a mixture G; S93: Grind the mixture G to obtain the coal-based powdered activated carbon.

10. The high-strength and high-specific-surface-area coal-based powdered activated carbon according to claim 9, characterized in that: The particle size of the coal-based powdered activated carbon prepared in S93 is 500 mesh.

Citation Information

Patent Citations

  • Method for adjusting pore structure of activated carbon

    CN102205961A

  • Tail gas continuous processing device utilizing alkaline activation to prepare activated carbon and tail gas continuous processing method thereof

    CN103599681A

  • Method for preparing coaly activated carbon by using fly ash or slag ash

    CN103626174A

  • Sargassum-based activated carbon and preparation method and application thereof

    CN104495837A

Cited By

  • A carbon-based powder adsorbent material and a method for preparing the same

    CN122916133A