Preparation method of surface porous Co2B compound
By preparing surface porous Co2B compounds and using their surface holes to absorb flue gas substances, the problems of high cost of high-temperature boiler pipeline materials and poor anti-flue gas erosion performance are solved, cost savings and performance improvements are achieved, and a cost-effective replacement is available. Strength alloy potential.
Patent Information
- Application Number
- CN202411179913.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing high-temperature service power station boiler pipeline materials are cost-effective in preparation, and they perform poorly in high-temperature flue gas erosion, and lack cost-effective alternative materials.
Using a preparation method for surface porous Co2B compounds, the hole depth is controlled to improve the resistance to dynamic flue gas corrosion by ball milling high-purity Co powder and B4C powder in a specific molar ratio and pressing the blank in a high-strength steel mold.
It significantly reduces the cost of material production and improves the resistance to high-temperature damage. The surface holes can absorb flue gas substances, which significantly improves the resistance to dynamic flue gas erosion. It has a high cost performance and can replace the expensive "Sitelli" alloy.
Smart Images

Figure CN119039005A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a surface porous Co2B compound. Background Art
[0002] For materials such as high-temperature service power station boiler pipes that are subjected to long-term high-temperature flue gas erosion, the "Stellite" alloy currently used at home and abroad has ideal resistance to high-temperature damage, but the preparation cost is relatively high. For many users and researchers involved in high-temperature wear conditions, it is currently expected to obtain a material with lower cost and better service performance. Obviously, the invention of a surface porous Co2B compound material that can absorb boiler flue gas, which improves the ability to resist dynamic flue gas erosion by absorbing and gathering flue gas substances in the surface pores during service, so as to replace the "Stellite" alloy or dense cobalt-boron compound materials has important innovative significance and engineering application value. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a surface porous Co2B compound capable of adsorbing boiler flue gas.
[0004] In order to achieve the above object, the present invention is implemented by adopting the following technical scheme:
[0005] A process for preparing a surface porous Co2B compound, characterized in that it comprises the following steps:
[0006] Steps:
[0007] (1) Co powder and B4C powder with a purity of not less than 99% are weighed in a molar ratio of 8:1 and placed in a ball mill and vacuumed;
[0008] (2) placing the ball mill jar in a ball mill for 5 to 10 hours, and quickly filling the taken-out Co and B4C mixed powder into a high-strength steel mold to press the green sheet, controlling the pressure to 100 MPa to 500 MPa, and holding the pressure for 5 to 10 minutes;
[0009] (3) When the green body is placed in a vacuum induction sintering furnace, vacuum is first drawn. When the maximum temperature reaches 950°C to 1200°C, oxygen is introduced for 10 min to 30 min for decarburization, and the temperature is kept for 10 hours to 30 hours. After sintering, the green body is cooled with the furnace to finally obtain a Co2B compound with controllable surface pore depth.
[0010] In the above process, the particle size of the Co powder is ≤50 μm; the particle size of the B4C powder is ≤50 μm.
[0011] The vacuum degree of the ball mill is less than 10 -1 Pa.
[0012] The vacuum degree of the vacuum sintering is less than 10-1 The temperature rise rate of the vacuum sintering is 1°C / sec to 5°C / sec.
[0013] The process of preparing the surface porous Co2B compound of the present invention is simple, and the production cost per kilogram is only 35% to 50% of that of the "Staly" alloy, thereby significantly saving production costs. The surface pore depth of the prepared Co2B compound is controllable, and it has excellent high temperature damage resistance. For example, in a dynamic flue gas damage test (100 hours) in a 700°C high temperature flue gas simulation erosion test machine, compared with the "Staly" material under the same test conditions, its surface thickness loss is significantly lower than that of the "Staly" alloy, with a significantly high cost-effectiveness, making it possible to use it to replace the currently used expensive "Staly" alloy.
[0014] The present invention can prepare a Co2B compound with controllable surface pore depth, which can adsorb and gather boiler flue gas substances through the surface pores to resist dynamic flue gas erosion. At the same time, since the flue gas substances gather in the pores, they can play a pinning role, which is conducive to the stable existence of flue gas substances on the surface of the Co2B compound, and can significantly improve the performance of resisting dynamic flue gas erosion. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a schematic flow chart of a method for preparing a surface porous Co2B compound according to an embodiment of the present disclosure;
[0016] Figure 2 This is a photo of the surface porous Co2B compound prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0017] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a surface porous Co2B compound, comprising:
[0018] Step S1, providing Co powder and B4C powder;
[0019] Step S2, putting the Co powder and the B4C powder into a ball mill and evacuating the mill;
[0020] Step S3, using the ball mill to ball mill the Co powder and the B4C powder to obtain a mixed powder;
[0021] Step S4, filling the mixed powder into a high-strength steel mold to press a green body, controlling the pressure and maintaining the pressure to obtain a green body;
[0022] Step S5, placing the green body into a vacuum induction sintering furnace and evacuating the furnace for vacuum sintering, introducing oxygen for decarburization when the highest temperature is reached, and cooling to obtain a surface porous Co2B compound.
[0023] Embodiment 1:
[0024] (1) Co powder and B4C powder with a purity of 99.9% and a powder size of 50 μm, respectively, were weighed in a molar ratio of 12:1 and placed in a ball mill and evacuated to a vacuum level of 10 -2 Pa;
[0025] (2) The ball mill jar was placed in a ball mill for 10 hours, and the Co and B4C mixed powder was quickly filled into a high-strength steel mold for compaction, the pressure was controlled at 500 MPa, and the pressure was maintained for 10 minutes;
[0026] (3) Place the green body in a vacuum induction sintering furnace and sinter at 1200°C (the vacuum degree during sintering is 10 -2 Pa. The heating rate of the sintering furnace is 1°C / second. ) and oxygen is introduced for 30 minutes, and the temperature is kept for 30 hours. After sintering, the furnace is cooled, and finally a Co2B compound with a surface hole depth of about 100μm to 300μm is obtained.
[0027] The surface porous Co2B sample obtained in this example The surface hole depth is about 121μm~173μm; for Stellite alloy The porous Co2B sample was put into a high-temperature flue gas simulation erosion test machine for dynamic flue gas damage test at 700°C for 100 hours. After the test, the sample was put into acetone for ultrasonic cleaning and then dried. The change in the height direction after damage was measured with a vernier caliper. The height reduction value of the sample before and after the test is shown in Table 1. It can be seen from the data in the table that the flue gas erosion resistance of the alloy prepared by the present invention is significantly improved, which is more than doubled. Figure 1 Shown is a photograph of the surface porous Co2B compound prepared in Example 1 of the present invention.
[0028] Table 1
[0029]
[0030]
[0031] Example 2
[0032] The process of this embodiment is the same as that of embodiment 1, except that some process parameters are different:
[0033] The purity and particle size of Co powder are 99% and 30μm respectively, and the purity and particle size of B4C powder are 99.9% and 50μm respectively. The ball milling time is 5 hours, and the accuracy of the ball mill is 10 -3 Pa; the green compact pressure is 100MPa, and the pressure is maintained for 10 minutes; the heating rate of the vacuum furnace during sintering is 5℃ / second, and the vacuum is first drawn for 10-3 Pa; when the sintering temperature reaches 950°C, oxygen is introduced for 10 minutes, and the sintering heat preservation time is 10 hours.
[0034] The obtained Co2B bulk sample has a porous surface (the surface pore depth is about 52μm to 72μm) With "Staly" alloy The comparison is shown in Table 2 (the experimental conditions are the same as in Example 1).
[0035] Table 2
[0036] "Steryl" alloy <![CDATA[Surface-porous Co2B]]> Height reduction value (μm) 93.6 56.1
[0037] Example 3
[0038] The process of this embodiment is the same as that of embodiment 1, except that some process parameters are different:
[0039] The purity and particle size of Co powder are 99.9% and 50μm respectively, and the purity and particle size of B4C powder are 99% and 20μm respectively. The ball milling time is 7 hours, and the accuracy of the ball mill is 10 -2 Pa; the green compact pressure is 300MPa, and the pressure is maintained for 7 minutes; the heating rate of the vacuum furnace during sintering is 3℃ / second, and the vacuum is first drawn for 10 -3 Pa; when the sintering temperature reaches 1050℃, oxygen is introduced for 20 minutes and the sintering heat preservation time is 20 hours.
[0040] The obtained Co2B bulk sample has a porous surface (the surface pore depth is about 83μm to 106μm). With "Staly" alloy The comparison is shown in Table 3 (the experimental conditions are the same as in Example 1).
[0041] Table 3
[0042] "Steryl" alloy <![CDATA[Surface-porous Co2B]]> Height reduction value (μm) 93.6 47.3
[0043] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.
Claims
1. A method for preparing a surface porous Co2B compound, characterized in that: The method comprises: Provide Co powder and B4C powder; The Co powder and the B4C powder are placed in a ball mill and vacuumized; Using the ball mill to ball mill the Co powder and the B4C powder to obtain a mixed powder; Filling the mixed powder into a high-strength steel mold for green compaction, controlling and maintaining the pressure to obtain a green body; The green body is placed in a vacuum induction sintering furnace and evacuated for vacuum sintering. When the highest temperature is reached, oxygen is introduced for decarburization. The green body is cooled to obtain a surface porous Co2B compound.
2. The method according to claim 1, characterized in that: The step of placing the Co powder and the B4C powder into a ball mill and evacuating the ball mill comprises: The Co powder and the B4C powder with a purity of not less than 99% are weighed at a molar ratio of 8:1, loaded into a ball mill and evacuated.
3. The method according to claim 2, characterized in that The vacuum degree of the ball mill is less than 10 -1 Pa.
4. The method according to claim 1, characterized in that: The method of ball milling the Co powder and the B4C powder using the ball mill comprises: The ball mill jar is placed in a ball mill for ball milling for 5 to 10 hours.
5. The method according to claim 1, characterized in that The step of filling the mixed powder into a high-strength steel mold and pressing the blank, controlling the pressure and maintaining the pressure comprises: Control the pressure to 100 MPa to 500 MPa; and / or, maintain the pressure for 5 min to 10 min.
6. The method according to claim 1, characterized in that The step of introducing oxygen to decarbonize when the maximum temperature is reached comprises: The maximum temperature is 950° C. to 1200° C.; and / or the oxygen introduction time is 10 min to 30 min.
7. The method according to any one of claims 1 to 6, characterized in that: The particle size of the Co powder is not greater than 50 μm.
8. The method according to any one of claims 1 to 6, characterized in that: The particle size of the B4C powder is not greater than 50 μm.
9. The method according to any one of claims 1 to 6, characterized in that: The vacuum degree of the vacuum sintering is less than 10 - 1 Pa.
10. The method according to any one of claims 1 to 6, characterized in that: The heating rate of the vacuum sintering is 1°C / sec to 5°C / sec.
Citation Information
Patent Citations
Flaky and porous cobalt boride powder and preparation method thereof
CN106430226A
Preparation method of WCoB-B<4>C ceramic matrix composite material
CN109351979A
Method for producing high-entropy alloy boride
RU2804391C1
Methods for manufacturing of cobalt boride coating layer on surface of steels by using a pack cementation process
US20130260160A1