Highlight universal water-based kaolin filler slurry as well as preparation method and application thereof
Through the use of high-light universal water-based kaolin filler slurry, the problem of low hiding power of dry film of water-based metal anticorrosion coatings is solved, and the cost reduction and gloss improvement are achieved. It is suitable for the stability and hiding power of water-based emulsion coatings.
Patent Information
- Application Number
- CN202411326094.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The dry film hiding power of water-based metal anticorrosion coatings is lower than that of wet films, resulting in a high sensitivity to the coating in the construction environment, and adding fillers or resins to increase hiding power will increase costs.
Using high-light universal aqueous kaolin filler slurry, the resin is coated with the dispersant of BYK194, NOPCALL-5180 and SN-1776 to form high-concentration kaolin particles with narrow particle size distribution, reducing viscosity and improving dispersion , combined with composite anti-deposition agent to form a stable structure, reducing the use of titanium dioxide and water.
It improves the dry film hiding power of the coating, reduces costs, enhances the gloss and storage stability of the coating, and is suitable for aqueous emulsion coatings.
Smart Images

Figure BDA0005055460690000051 
Figure BDA0005055460690000061 
Figure BDA0005055460690000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a high-gloss universal water-based kaolin filler slurry and a preparation method and application thereof. Background Art
[0002] The water in water-based metal anticorrosion coatings takes more time to evaporate and dry, and is sensitive to the construction environment. The curing process is greatly affected by temperature and humidity. Unsuitable environmental conditions may be unfavorable for the formation of paint films. During the construction of the paint, the wet film contains a large amount of solvent or water. These liquid components help to disperse the pigment particles and reduce the aggregation between the pigments, so that the paint can cover the base material more effectively. As the paint dries, the solvent or water gradually evaporates, and the pigment particles are rearranged and may aggregate, resulting in a decrease in hiding power. Therefore, the hiding power of the dry film is usually lower than that of the wet film. The reason is that the difference in refractive index between the pigment in the paint and the paint matrix (such as water or resin) affects the hiding power. When the paint is wet, the pigment particles are surrounded by water, and after drying, the pigment particles are surrounded by resin or air. Due to the different refractive indices of water and resin or air, this affects the way light passes through the coating film, thereby affecting the hiding power. Especially when pure white or light white paint is applied, the color or flaws of the primer are no longer visible when the topcoat is sprayed on the wet film, but the base color or flaws of the primer are revealed after the topcoat film dries.
[0003] In order to ensure that the topcoat has good dry hiding power to cover the flaws or color of the primer underneath, a large amount of titanium dioxide is often added to the topcoat or a thicker topcoat is sprayed, which leads to higher costs. The topcoat of water-based metal anti-corrosion coatings requires high protective and decorative properties, and most of them have high requirements for gloss, so the pigment-to-base ratio is generally very low. For this reason, only a small amount of filler powder is added to the formula, mostly resin, solvent, and water.
[0004] Since adding more resin and solvent to water-based metal anti-corrosion coatings will increase product costs, and adding more water will slow down the volatilization of water and increase the amount of thickener. Therefore, it is of great significance to develop a universal filler slurry with strong versatility, better dispersion effect, low impact on coating gloss and significant improvement in coating dry hiding power. Summary of the invention
[0005] The present invention provides a high-gloss universal water-based kaolin filler slurry and a preparation method and application thereof, so as to provide a filler slurry with strong versatility, small particle size, uniform dispersion, and low impact on the gloss of the paint film, while effectively improving the dry film hiding power of the paint film, reducing the addition amount of titanium dioxide, resin emulsion and water, and reducing costs.
[0006] In order to solve the above technical problems, one of the purposes of the present invention is to provide a high-gloss universal water-based kaolin filler slurry, comprising the following components in parts by weight:
[0007] Kaolin powder: 50-60 parts;
[0008] Dispersant: 1-3 parts;
[0009] Coating resin: 1-4 parts;
[0010] Composite anti-settling agent: 0-3 parts;
[0011] Solvent: 1-5 parts;
[0012] Defoaming agent A: 0.3-1 part;
[0013] Wetting agent A: 0.2-0.5 parts;
[0014] The dispersant comprises BYK194, NOPCALL-5180 and SN-1776 in a mass ratio of (2-6): (2-6): (2-6), and the coating resin comprises THYON PH729, THYON SRT3069, THYON SR675 and THYON SR705 in a mass ratio of (2-8): (2-8): (2-8): (2-8).
[0015] By adopting the above scheme, the viscosity of high-concentration kaolin slurry is mainly related to its internal structure and the interaction between particles. At high concentrations, the contact between kaolin particles becomes more frequent, and the interaction force between particles is enhanced, resulting in an increase in the viscosity of the fluid. The shape and surface characteristics of kaolin particles will also affect their dispersion state and interaction in water. Irregular particle shapes and rough surfaces may increase the friction between particles. The dispersant in the kaolin filler slurry of the present application adopts a compound of BYK194, NOPCALL-5180 and SN-1776. The various active groups of the dispersant with positive and negative charges are adsorbed on the surface of fine kaolin particles, and hydrogen bonds are formed with functional groups such as hydroxyl (-Si(Al)-OH), silicon-oxygen tetrahedron (-Si-O-Al-) and aluminum-oxygen octahedron (-Si(Al)-O) on the surface of kaolin to form an anchoring effect, thereby activating the powder. The dispersant can form a steric hindrance effect, effectively reducing the irregular shape and rough surface of the particles, thereby effectively reducing the viscosity of the kaolin filler slurry under high shear force, and the slurry particle size is small, which is conducive to dispersion in the subsequent aqueous emulsion.
[0016] In addition, the coating resin added in the present application is a modified acrylic resin, and the dispersant carries numerous hydrogen bond donor and acceptor chain segments. The solvated chain segments in the dispersant extend in the coating resin to form a polymer chain segment barrier layer of a certain thickness, which prevents the aggregation and agglomeration between the powder particles, making the kaolin particles smaller in size. The particle size of the kaolin slurry has a narrow particle size distribution, and the gloss will not be reduced when a large amount is added to the coating. At the same time, the dry film hiding power of the paint film is improved, and the use of titanium dioxide is reduced.
[0017] As a preferred embodiment, the composite anti-settling agent comprises RHEOBYK-420, BYK R 605, RHEOBYK-H7625VF and AEROSIL 200 in a mass ratio of (1-4):(1-4):(1-4):(1-4).
[0018] By adopting the above scheme, the composite anti-settling agent of the present application forms micelles in the aqueous phase system, and the hydrophobic end is adsorbed together with the hydrophobic structure in the dispersant and the coating resin, which synergistically solves the difficulty of anti-settling and poor storage stability, and forms a three-dimensional anti-settling network structure. The hydrophilic end of the composite anti-settling agent is thickened by hydrogen bond hydration, and the viscosity of the system is adjusted, which can improve the stability of the filler slurry system and withstand long-term and high-temperature storage.
[0019] As a preferred embodiment, the solvent is at least one of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; the defoamer A is at least one of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024; and the wetting agent A is at least one of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, and SURFYNOL104E.
[0020] In order to solve the above technical problems, the second object of the present invention provides a method for preparing a high-gloss general-purpose water-based kaolin filler slurry, comprising the following steps:
[0021] (1) adding the water, solvent, dispersant, defoamer and wetting agent in sequence and mixing them evenly, adding kaolin powder and dispersing them evenly, and then grinding them with a horizontal mill to make the slurry particle size reach 0.8um≥95%, thereby obtaining a kaolin fine raw material slurry;
[0022] (2) Grinding the kaolin fine raw material slurry, adding the coating resin and the composite anti-settling agent, and mixing them evenly to obtain a kaolin filler slurry.
[0023] As a preferred embodiment, in step (1), the grinding medium balls include medium balls with diameters of 3 mm, 1.5 mm and 0.8 mm in a mass ratio of 1:2:2, the grinding speed is 500-800 rpm, the grinding time is 1-3 h, and the grinding temperature is less than 70°C.
[0024] In order to solve the above technical problems, the third object of the present invention provides an application of a high-gloss general-purpose water-based kaolin filler slurry in the field of preparing water-based emulsion coatings.
[0025] In order to solve the above technical problems, the fourth object of the present invention provides a water-based emulsion coating, including a high-gloss general-purpose water-based kaolin filler slurry with a mass fraction of 5wt%-20wt%.
[0026] As a preferred embodiment, the invention comprises the following components in parts by weight:
[0027] Aqueous emulsion: 50-70 parts;
[0028] Defoaming agent B: 0.3-0.8 parts;
[0029] Wetting agent B: 0.2-0.6 parts;
[0030] Leveling agent: 0.1-0.3 parts;
[0031] Film-forming aid: 2-6 parts;
[0032] Water-based titanium dioxide slurry: 5-15 parts;
[0033] High gloss general purpose water-based kaolin filler slurry: 10-20 parts;
[0034] Water: 10-20 parts.
[0035] By adopting the above scheme, the kaolin filler slurry of the present application is added to the water-based emulsion paint. Since the kaolin particles have a narrow particle size distribution, a small particle size and a low viscosity, a large amount of addition does not affect the gloss of the paint film. At the same time, the kaolin filler slurry can also improve the dry film hiding power of the paint, reduce the amount of titanium dioxide slurry added, and reduce costs. The higher concentration of kaolin filler slurry can also reduce the content ratio of water-based emulsion and water in the system, and increase the volatilization rate of water in the paint film. In addition, the kaolin filler slurry has a stable particle size and can withstand high temperature environments and long-term storage without stratification, which can improve the storage stability of the paint.
[0036] As a preferred embodiment, the film-forming aid is C12 alcohol ester.
[0037] As a preferred embodiment, the aqueous emulsion is an aqueous acrylic emulsion.
[0038] As a preferred embodiment, the defoamer B is at least one of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024, and the wetting agent B is at least one of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, and SURFYNOL104E.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. The dispersant in the kaolin filler slurry of the present application is a compound of BYK194, NOPCALL-5180 and SN-1776. The various active groups of the positive and negative charges of the dispersant are adsorbed on the surface of fine kaolin particles during the grinding process, and hydrogen bonds are formed with functional groups such as hydroxyl groups, silicon-oxygen tetrahedrons and aluminum-oxygen octahedrons on the surface of kaolin to generate an anchoring effect, thereby activating the powder, effectively reducing the irregular shape and rough surface of the particles, and thus effectively reducing the viscosity of the kaolin filler slurry under high shear force. The slurry has a small particle size, which is conducive to dispersion in the subsequent aqueous emulsion and does not affect the gloss of the aqueous emulsion.
[0041] 2. The coating resin added in this application is a modified acrylic resin, and the dispersant carries numerous hydrogen bond donor and acceptor segments. The solvated segments in the dispersant extend in the coating resin to form a polymer segment barrier layer of a certain thickness, which prevents the aggregation and agglomeration between the powder particles, making the kaolin particles smaller in size. The particle size of the kaolin slurry has a narrow particle size distribution, and the gloss will not be reduced when a large amount is added to the paint. At the same time, the dry film hiding power of the paint film is improved, and the use of titanium dioxide is reduced.
[0042] 3. The composite anti-settling agent of the present application forms micelles in the aqueous phase system, and the hydrophobic end is adsorbed together with the hydrophobic structure in the dispersant and the coating resin to form a three-dimensional anti-settling network structure, which synergistically solves the problems of difficult anti-settling and poor storage stability, can improve the stability of the filler slurry system, and can withstand long-term and high-temperature storage. The water-based kaolin filler slurry has a higher effective solid concentration and better cost-effectiveness. DETAILED DESCRIPTION
[0043] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Table 1 - Sources of raw materials used in the examples and comparative examples of this application
[0045]
[0046]
[0047] Example 1
[0048] A high-gloss universal water-based kaolin filler slurry comprises 3wt% propylene glycol solvent, 0.5wt% TEGO902W defoamer, 0.3wt% BYK346 wetting agent, 50wt% calcined kaolin powder, 2wt% coating resin, 1.2wt% dispersant, 1wt% composite anti-settling agent and the balance deionized water, wherein the coating resin comprises 0.8wt% of THYON PH729, 0.6wt% of THYON SRT3069, 0.4wt% of THYON SR675 and 0.2wt% of THYON SR705 in terms of the mass fraction of the filler slurry, and the composite anti-settling agent comprises 0.2wt% of RHEOBYK-420, 0.1wt% of BYK R 605, 0.4wt% of RHEOBYK-H7625VF and 0.3wt% of AEROSIL 200, the dispersant includes 0.4wt% BYK194, 0.6wt% NOPCALL-5180 and 0.2wt% SN-1776, accounting for 0.4wt% of the filler slurry mass fraction.
[0049] The method for preparing the above-mentioned high-gloss universal water-based kaolin filler slurry comprises the following steps:
[0050] (1) Deionized water, solvent, dispersant, defoamer, and wetting agent are sequentially added to a stirring kettle and mixed evenly. After adding kaolin powder, the mixture is dispersed at a high speed of 1000 rpm for 30 minutes. The mixture is then ground in a horizontal mill. The grinding medium balls include 3 mm, 1.5 mm, and 0.8 mm medium balls with a mass ratio of 1:2:2. The grinding speed is 600 rpm, the grinding time is 2 h, and the grinding temperature is less than 70° C. The final kaolin slurry particle size reaches 0.8 μm ≥ 95%, thereby obtaining a kaolin fine raw material slurry.
[0051] (2) After the particle size reaches the standard, the coating resin and the composite anti-settling agent are added to the kaolin fine raw material slurry, and the mixture is mixed evenly to obtain a kaolin filler slurry.
[0052] Example 2
[0053] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that the dispersant includes 0.2wt% BYK194, 0.4wt% NOPCALL-5180 and 0.6wt% SN-1776 in the filler slurry.
[0054] Example 3
[0055] A high-gloss universal water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that the dispersant includes 0.6wt% BYK194, 0.2wt% NOPCALL-5180 and 0.4wt% SN-1776 in the filler slurry.
[0056] Example 4
[0057] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that the dispersant includes 0.6wt% BYK194, 0.4wt% NOPCALL-5180 and 0.2wt% SN-1776 in the filler slurry.
[0058] Comparative Example 1
[0059] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 1, except that the dispersant includes SN-5040 accounting for 1.2 wt% of the filler slurry.
[0060] Comparative Example 2
[0061] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 1, except that the dispersant includes TEGO760W accounting for 1.2 wt% of the filler slurry.
[0062] Comparative Example 3
[0063] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 1, except that the dispersant includes 1.2 wt% of NOPCALL-5180 in the filler slurry.
[0064] The brushing sensation and viscosity of the kaolin fine raw material slurry before grinding and the particle size properties of the kaolin filler slurry of the above-mentioned Examples 1-4 and Comparative Examples 1-3 were detected and recorded, and the kaolin filler slurries of Examples 1-4 and Comparative Examples 1-3 were respectively applied to aqueous emulsions to prepare test samples, and the blank group samples used an equal amount of aqueous emulsion to replace the kaolin filler slurry, and were tested, including the following steps:
[0065] (1) The slurry of kaolin fine raw material before grinding is subjected to a slurry ...
[0066] (2) preparing a water-based emulsion coating, taking 60 g of Wanhua Chemical's model 0626 water-based acrylic emulsion, adding 0.5 g of model TEGO902W defoamer, 0.3 g of model BYK346 wetting agent, 0.2 g of model TEGO450 leveling agent, 4 g of C12 alcohol ester film-forming aid, 10 g of Guangdong Kedi W1006-SI water-based titanium dioxide slurry and 10 g of water, then adding 15 g of kaolin filler slurry, mixing evenly to prepare a water-based emulsion coating;
[0067] (3) The aqueous emulsion coating was used to make a film on a glass plate with a film thickness of 100 μm;
[0068] (3) The film samples were tested for gloss and dry film reflectivity. The gloss test was carried out in accordance with GB / T9754-2007 "Paints and varnishes - Determination of specular gloss at 20°, 60° and 85° of paint films without metallic pigments". The reflectivity test method was carried out in accordance with GB / T 23981.1-2019 "Determination of hiding power of paints and varnishes - Part 1: Determination of contrast ratio of white and light-colored paints". The test results are shown in Table 2 below.
[0069] Table 2 - Performance test results of aqueous emulsions prepared with kaolin fillers in Examples 1-4 and Comparative Examples 1-3 of the present application
[0070]
[0071]
[0072] As shown in Table 2, compared with the blank group without kaolin filler slurry, the dispersants in the kaolin filler slurries of Examples 1-4 of the present application are BYK194, NOPCALL-5180 and SN-1776, which are compounded and added in proportion. The shape and surface characteristics of kaolin particles will also affect their dispersion state and interaction in water. The present application utilizes the various active groups of positive and negative charges of the dispersant to be adsorbed on the surface of fine kaolin particles, and the hydroxyl groups (-Si(Al)-OH), silicon-oxygen tetrahedrons (-Si-O-Al-) and aluminum-oxygen octahedrons (-Si-O-Al-) on the surface of the kaolin are bonded to the surface of the kaolin particles during the grinding process. The dispersant can form a steric hindrance effect, effectively reduce the irregular shape and rough surface of the particles, and then effectively reduce the viscosity of the kaolin filler slurry under high shear force, which is beneficial to reduce the kaolin particle size and disperse it evenly in the aqueous emulsion, improve the dry hiding power of the paint film, and have little effect on the gloss of the paint film; at the same time, compared with the single dispersant component in the kaolin filler slurry of comparative examples 1-3, the films prepared by adding the compound dispersant in Examples 1-4 of the present application have higher gloss and dry film reflectivity.
[0073] Example 5
[0074] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 1, except that kaolin powder accounts for 60wt% of the filler slurry.
[0075] Example 6
[0076] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 2, except that kaolin powder accounts for 60wt% of the filler slurry.
[0077] Example 7
[0078] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps as those of Example 3 as well as the reagents, equipment and process parameters used in each step, except that kaolin powder accounts for 60wt% of the filler slurry by mass.
[0079] Example 8
[0080] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 4, except that kaolin powder accounts for 60wt% of the filler slurry.
[0081] Comparative Example 4
[0082] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 5, except that the dispersant includes SN-5040 accounting for 1.2 wt% of the filler slurry.
[0083] Comparative Example 5
[0084] A high-gloss universal water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 5, except that the dispersant includes TEGO760W accounting for 1.2wt% of the filler slurry.
[0085] Comparative Example 6
[0086] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 5, except that the dispersant includes 1.2 wt% of NOPCALL-5180 in the filler slurry.
[0087] The brush feel and viscosity of the kaolin fine raw material slurry before grinding and the particle size properties of the kaolin filler slurry of the above-mentioned Examples 5-8 and Comparative Examples 4-6 were detected and recorded, and the kaolin filler slurries of Examples 5-8 and Comparative Examples 4-6 were respectively applied to aqueous emulsions to prepare test samples, and film gloss and dry film reflectivity tests were performed. The operating steps for preparing aqueous emulsion coatings and film samples are the same as described above and will not be repeated here. Among them, the blank group samples used an equal amount of aqueous emulsion to replace the kaolin filler slurry. The test results are shown in Table 3 below.
[0088] Table 3 - Performance test results of aqueous emulsions prepared with kaolin fillers in Examples 5-8 and Comparative Examples 4-6 of the present application
[0089]
[0090] As shown in Table 3, the kaolin concentration in the filler slurry of Comparative Examples 4-5 is increased, resulting in more frequent contact between particles and enhanced interaction forces, which increases the viscosity of the filler slurry, creates a strong sense of stagnation and makes it difficult to grind. The kaolin particles are unevenly distributed and have a large particle size, which results in a serious decrease in the gloss of the final prepared film. Although the filler slurries of Examples 5-8 of the present application have a certain degree of increased viscosity, the sense of stagnation is relatively mild and does not affect grinding. The prepared film has improved dry hiding power and a higher gloss than that of Comparative Examples 4-6, which can be maintained at a relatively high level.
[0091] Example 9
[0092] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, the reagents, equipment and process parameters used in each step are the same as those in Example 7, except that the coating resin includes 0.2wt% of THYON PH729, 0.4wt% of THYON SRT3069, 0.6wt% of THYON SR675 and 0.8wt% of THYONSR705, accounting for 0.2wt% of the mass fraction of the filler slurry.
[0093] Example 10
[0094] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, the reagents, equipment and process parameters used in each step are the same as those in Example 7, except that the coating resin includes 0.4wt% of THYON PH729, 0.6wt% of THYON SRT3069, 0.2wt% of THYON SR675 and 0.8wt% of THYONSR705, accounting for 0.4wt% of the mass fraction of the filler slurry.
[0095] Embodiment 11
[0096] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, the reagents, equipment and process parameters used in each step are the same as those in Example 7, except that the coating resin includes 0.6wt% of THYON PH729, 0.2wt% of THYON SRT3069, 0.8wt% of THYON SR675 and 0.4wt% of THYONSR705, accounting for 0.6wt% of the mass fraction of the filler slurry.
[0097] Comparative Example 7
[0098] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which has the same steps as those of Example 7 as well as the reagents, equipment and process parameters used in each step, except that the coating resin includes 2 wt% of Xinghengtai 518H by mass fraction of the filler slurry.
[0099] Comparative Example 8
[0100] A high-gloss general-purpose water-based kaolin filler slurry, the preparation method of which, each step and the reagents, equipment and process parameters used in each step are the same as those in Example 7, except that the coating resin includes Lihuayi 702 accounting for 2 wt% of the filler slurry.
[0101] Comparative Example 9
[0102] A high-gloss universal water-based kaolin filler slurry, the preparation method of which has the same steps, reagents, equipment and process parameters as those in Example 7, except that the coating resin includes 2 wt% of THYON SR675 in the filler slurry.
[0103] The kaolin filler slurry of Examples 7, 9-11 and Comparative Examples 7-9 was respectively applied to aqueous emulsion to prepare test samples, and the film gloss and dry film reflectivity tests were performed. The preparation steps of aqueous emulsion coatings and film samples are the same as described above and will not be repeated here. Among them, the blank group samples used an equal amount of aqueous emulsion to replace the kaolin filler slurry. The difference between the experimental group and the film sample of Example 10 is that 2g of aqueous titanium dioxide slurry was replaced by water. The test results are shown in Table 4 below.
[0104] At the same time, the film samples of the blank group, the experimental group and Example 10 were subjected to hardness (pencil method), adhesion (grid method) and solid content tests. The solid content test was carried out in accordance with the standard GB / T 1725-2007 "Determination of non-volatile content of paints, varnishes and plastics". The solid content test conditions were 105°C / 1h. The test results are shown in Table 4 below.
[0105] Table 4 - Performance test results of aqueous emulsions prepared with kaolin fillers in Examples 7, 9-11 and Comparative Examples 7-9 of the present application
[0106] As shown in Table 4, compared with the single coating resin in Comparative Examples 7-9, the coating resin added in Examples 7 and 9-11 of the present application is a modified acrylic resin, and the dispersant added at the same time has segments of numerous hydrogen bond donors and acceptors. The solvated segments in the dispersant extend in the coating resin to form a polymer segment barrier layer of a certain thickness, which prevents aggregation and agglomeration between powder particles, makes the kaolin particles smaller, and improves the glossiness of the prepared water-based paint film.
[0107] Example 12
[0108] A high-gloss universal water-based kaolin filler slurry, wherein the steps of the preparation method and the reagents, equipment and process parameters used in the steps are the same as those in Example 10, except that the composite anti-settling agent comprises 0.1wt% of RHEOBYK-420, 0.2wt% of BYK R 605, 0.3wt% of RHEOBYK-H7625VF and 0.4wt% of AEROSIL 200, accounting for 0.1wt% of the mass fraction of the kaolin filler slurry.
[0109] Embodiment 13
[0110] A high-gloss universal water-based kaolin filler slurry, wherein the steps of the preparation method and the reagents, equipment and process parameters used in the steps are the same as those in Example 10, except that the composite anti-settling agent comprises 0.2 wt% of RHEOBYK-420, 0.1 wt% of BYK R 605, 0.3 wt% of RHEOBYK-H7625VF and 0.4 wt% of AEROSIL 200, accounting for 0.2 wt% of the mass fraction of the kaolin filler slurry.
[0111] Embodiment 14
[0112] A high-gloss universal water-based kaolin filler slurry, wherein the steps of the preparation method and the reagents, equipment and process parameters used in the steps are the same as those in Example 10, except that a composite anti-settling agent is further added, and the composite anti-settling agent comprises 0.1wt% of RHEOBYK-420, 0.2wt% of BYK R 605, 0.4wt% of RHEOBYK-H7625VF and 0.3wt% of AEROSIL 200, accounting for 0.1wt% of the mass fraction of the kaolin filler slurry.
[0113] Comparative Example 10
[0114] A high-gloss universal water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 10, except that the composite anti-settling agent includes DISPARLON AQ-607 accounting for 1wt% of the mass fraction of the kaolin filler slurry.
[0115] Comparative Example 11
[0116] A high-gloss universal water-based kaolin filler slurry, the preparation method of which, in each step and as well as the reagents, equipment and process parameters used in each step, are the same as those in Example 10, except that the composite anti-settling agent includes 1 wt% of Guojian SHV by mass fraction of the kaolin filler slurry.
[0117] Comparative Example 12
[0118] A high-gloss universal water-based kaolin filler slurry, the preparation method of which, the steps and the reagents, equipment and process parameters used in each step are the same as those in Example 10, except that the composite anti-settling agent includes RHEOBYK-420 accounting for 1 wt% of the mass fraction of the kaolin filler slurry.
[0119] The kaolin filler slurry of the above-mentioned Examples 10, 12-14 and Comparative Examples 10-12 was subjected to a 50°C shaking table treatment for 7 days with a swing amplitude of 26 mm in diameter and a swing frequency of 75 rpm to observe the properties of the filler slurry. At the same time, a 55°C hot storage treatment for 30 days was carried out to observe the properties of the filler slurry and detect and record the percentage decrease in the slurry particle size less than 0.8 μm before and after the hot storage of the filler slurry. The test results are shown in Table 5 below.
[0120] Table 5 - Performance test results of kaolin fillers in Examples 10, 12-14 and Comparative Examples 10-12 of the present application
[0121] As shown in Table 5, compared with the single anti-settling agent in Comparative Examples 10-12, Examples 10 and 12-14 of the present application use a composite anti-settling agent. The composite anti-settling agent forms micelles in the aqueous phase system, and the hydrophobic end is adsorbed together with the dispersant and the hydrophobic structure in the coating resin to form a three-dimensional anti-settling network structure. The hydrophilic end of the composite anti-settling agent is thickened by hydrogen bond hydration to adjust the viscosity of the system, thereby improving the stability of the filler slurry system and being able to withstand long-term and high-temperature storage.
[0122] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A high-gloss general-purpose water-based kaolin filler slurry, characterized in that: It comprises the following components in parts by weight: Kaolin powder: 50-60 parts; Dispersant: 1-3 parts; Coating resin: 1-4 parts; Composite anti-settling agent: 0-3 parts; Solvent: 1-5 parts; Defoaming agent A: 0.3-1 part; Wetting agent A: 0.2-0.5 parts; The dispersant comprises BYK194, NOPCALL-5180 and SN-1776 in a mass ratio of (2-6): (2-6): (2-6), and the coating resin comprises THYON PH729, THYON SRT3069, THYON SR675 and THYON SR705 in a mass ratio of (2-8): (2-8): (2-8): (2-8).
2. A high-gloss universal water-based kaolin filler slurry as claimed in claim 1, characterized in that: The composite anti-settling agent comprises RHEOBYK-420, BYK R 605, RHEOBYK-H7625VF and AEROSIL 200 in a mass ratio of (1-4):(1-4):(1-4):(1-4).
3. The high-gloss universal water-based kaolin filler slurry according to claim 1, characterized in that: The solvent is at least one of ethanol, propylene glycol, ethylene glycol butyl ether, and diethylene glycol monobutyl ether; the defoamer A is at least one of BYK022, BYK028, TEGO901W, TEGO902W, NOPTAM-398, NOPTAM-1311, and SN-6024; and the wetting agent A is at least one of BYK-346, BYK-345, TEGO270, TEGO4100, SURFYNOL465, and SURFYNOL104E.
4. A method for preparing a high-gloss general-purpose water-based kaolin filler slurry as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: (1) adding the water, solvent, dispersant, defoamer and wetting agent in sequence and mixing them evenly, adding kaolin powder and dispersing them evenly, and then grinding them with a horizontal mill to make the slurry particle size reach 0.8um≥95%, thereby obtaining a kaolin fine raw material slurry; (2) Grinding the kaolin fine raw material slurry, adding the coating resin and the composite anti-settling agent, and mixing them evenly to obtain a kaolin filler slurry.
5. The method for preparing a high-gloss general-purpose water-based kaolin filler slurry according to claim 4, characterized in that: In step (1), the grinding medium balls include medium balls with diameters of 3 mm, 1.5 mm and 0.8 mm in a mass ratio of 1:2:2, the grinding speed is 500-800 rpm, the grinding time is 1-3 hours, and the grinding temperature is less than 70°C.
6. Use of the high-gloss universal water-based kaolin filler slurry as claimed in any one of claims 1 to 3 in the field of preparing water-based emulsion coatings.
7. A water-based emulsion paint, characterized in that: The invention comprises 5wt%-20wt% of the high-gloss universal water-based kaolin filler slurry as described in any one of claims 1 to 6.
8. A water-based emulsion paint as claimed in claim 7, characterized in that: It includes the following components in parts by weight: Aqueous emulsion: 50-70 parts; Defoaming agent B: 0.3-0.8 parts; Wetting agent B: 0.2-0.6 parts; Leveling agent: 0.1-0.3 parts; Film-forming aid: 2-6 parts; Water-based titanium dioxide slurry: 5-15 parts; High gloss general purpose water-based kaolin filler slurry: 10-20 parts; Water: 10-20 parts.
9. A water-based emulsion paint as claimed in claim 8, characterized in that: The film-forming aid is C12 alcohol ester.
10. A water-based emulsion paint as claimed in claim 8, characterized in that: The aqueous emulsion is an aqueous acrylic emulsion.
Citation Information
Patent Citations
Highlight universal water-based nuclear titanium dioxide slurry and preparation method thereof
CN117924972A