Production process of torsion-free plain cloth

Through knitting machine woven and tension-free alkali shrinkage treatment technology, combined with the cross-linking alkali shrinkage additive, the torque problem of plain jerseys in the production process is solved, the production of torque-free plain jerseys is realized, and its dimensional stability and application are improved. Range, can replace traditional woven fabrics.

CN119061566AInactive Publication Date: 2024-12-03NINGBO BETTER TEXTILE&GARMENTS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411528558.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing plain jerseys are prone to torque during production, which leads to distortion, deformation, irregular folds or inability to lay the fabric during processing, wearing and use, affecting its dimensional stability and service life.

Method used

After woven, the alkali shrinkage treatment is carried out by using a knitting machine, combined with the alkali shrinkage additive with cross-linking effect, through the tension-free alkali shrinkage treatment and subsequent dyeing and finishing process, the fabric is fully in contact with the alkali liquid and a tight cross-linking network is formed. Eliminate stress accumulation and improve dimensional stability and wrinkle resistance of fabrics.

Benefits of technology

The production of torque-free plain jerseys has been achieved, and the torque test results can reach <0.5%, which is comparable to that of traditional woven fabrics, ensuring excellent dimensional stability and torque-free characteristics, expanding the application range, and being able to replace traditional woven fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of textile production, and relates to a production process of torsion-free plain cloth. The production process comprises the following steps: weaving yarns by using a knitting machine to obtain blank cloth; carrying out alkali shrinkage treatment on the blank cloth, and then carrying out a subsequent dyeing and finishing process to obtain the finished product torsion-free plain cloth. According to the production process, optimized weaving process parameters are combined with an innovative tension-free novel alkali shrinkage treatment technology, so that the compactness of the produced torsion-free plain cloth reaches an excellent level. Under optimal parameter setting, the torsion test result is infinitely close to zero, the performance of the woven fabric is equivalent to that of the traditional woven fabric, the woven fabric with the same thickness can be completely replaced, and excellent dimensional stability and torsion-free characteristics are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile production, and relates to a production process of a non-torsion plain weave cloth. Background Art

[0002] Plain fabric is widely used in daily life due to its simple structure, uniform texture, easy dyeing and printing. This fabric is an ideal choice for many home textiles and clothing due to its smooth feel, good air permeability, and easy cleaning and maintenance. Compared with woven fabrics, the production process of knitted plain fabric is simpler and the production speed is fast, which makes it have obvious advantages in cost control and rapid response to market changes.

[0003] In terms of household items, plain fabric is often used to make sheets, pillowcases, tablecloths and curtains. Its smooth surface is not only beautiful, but also easy to clean, which is very suitable for environments with frequent daily use. Especially in summer, plain fabric has become an ideal material for making bedding due to its good breathability and moisture absorption, helping people stay cool and comfortable in hot weather. In the field of clothing, plain fabric is very suitable for making T-shirts, underwear, pajamas and children's clothing due to its lightness and softness. These clothes require comfortable and skin-friendly fabrics, and plain fabric just meets these needs. In addition, plain fabric can also create colorful patterns and colors through advanced printing and dyeing technology to meet the growing personalized needs of consumers.

[0004] Torque (Twist or Skew) in textiles refers to the twisting or tilting of fabrics during processing, handling or use. Specifically, torque refers to the rotation or deviation of fabrics in one direction relative to another. This phenomenon can occur in multiple links such as weaving, dyeing, printing, sewing, etc., and will affect the appearance and performance of the fabric. Plain weave fabrics are usually connected together by a ring structure formed by continuous yarns, which gives it a certain degree of stretch and elasticity. During the production process, knitting machines (such as large circular knitting machines) are used to pass yarns through needles to form a continuous coil structure. Due to its structural characteristics, plain weave fabrics that have not been specially treated will show a certain tendency to twist, causing the fabric to twist or rotate during processing or wearing, especially in wet conditions. In contrast, woven fabrics are composed of vertically interwoven warp and weft yarns to form a stable flat grid structure. Due to the stability of its structure, woven fabrics have less or almost no torque in most cases, which means that woven fabrics are less likely to twist during processing and wearing, and have better dimensional stability.

[0005] For clothing manufacturers, if the plain fabric has a large torque, the fabric may twist or deform during the cutting and sewing process, resulting in asymmetric or ill-fitting finished garments. In household items such as bed sheets and curtains, if the plain fabric used has a torque problem, after a period of use, you may find that these items have irregular wrinkles or cannot be laid flat. Plain fabrics with high torque also need to be washed and ironed with extra care, otherwise they may shrink or deform after washing, and it will take more time and effort to iron them to restore their original appearance.

[0006] In order to overcome these problems, the textile industry is actively developing new technologies, striving to reduce the torque problem and improve the dimensional stability of knitted plain fabrics while maintaining the original advantages of knitted plain fabrics to better meet market demand. Summary of the invention

[0007] The present invention aims at the above problems existing in the prior art and provides a production process of a non-torsion plain weave fabric.

[0008] One object of the present invention is achieved by the following technical solutions:

[0009] A production process for a non-torsion plain weave fabric comprises the following steps: using a knitting machine to weave yarn to obtain a blank fabric; subjecting the blank fabric to an alkali shrinkage treatment, and then to a subsequent dyeing and finishing process to obtain a finished product of the non-torsion plain weave fabric.

[0010] Preferably, the knitting machine includes the following parameters: diameter of 30-50 inches, needle cylinder density of 30-50G, total number of needles of 2500-5000N, and counterclockwise weaving. That is, the diameter of the knitting machine working cylinder is 30-50 inches; the number of needles per inch is 30-50 needles, and the more needles, the finer the woven fabric; the total number of needles in one circle of the knitting machine is 2500-5000 needles.

[0011] More preferably, the knitting machine has a diameter of 30 to 40 inches, a needle cylinder density of 30 to 40G, and a total number of needles of 2500 to 3000N.

[0012] Preferably, the yarn length of the yarn is 9-11 cm / 50 N, that is, under a tension of 50 N, the length of the yarn is 9-11 cm.

[0013] Preferably, the woven structure is a single-sided plain weave structure.

[0014] Single jersey is a common knitted fabric structure with a simple interlacing pattern consisting of basic loops formed by yarn. The characteristic of this structure is that the front and back sides look the same or similar, so it is called single jersey structure. Each yarn is formed into a closed loop by crochet, and these loops are connected to each other in the horizontal and vertical directions, forming the basic structure of the fabric. The loops of each row are continuously formed by the same yarn, and the loops of two adjacent rows are interlocked together to form a continuous chain structure. The front and back sides of the fabric look very similar, usually showing a uniform texture and appearance.

[0015] Preferably, after the weaving is completed, the blank cloth needs to be singed, and the burner temperature during the singeing process is 1100-1200° C. and the speed is 80-95 m / min.

[0016] Preferably, the alkali shrinkage treatment comprises: immersing the raw fabric in an alkali agent and adding an alkali shrinkage aid for alkali shrinkage treatment, so that the tensile tension of the raw fabric is 0, and the treatment speed is 10-30 yards / min. During the alkali shrinkage process, ensure that the fabric is fully contacted with the solution and evenly treated, and do not allow the fabric to be stretched during the treatment process to avoid dimensional changes.

[0017] Preferably, the alkali agent is a sodium hydroxide solution, the temperature of the alkali agent is 25-35°C, and the concentration is 25-45°Bè (Baume, commonly used to measure the concentration of a solution in the textile industry).

[0018] Alkali shrinkage treatment (also called mercerizing treatment) is mainly used in fabric processing. It allows the fibers to fully swell and shrink in the alkali solution, thereby changing the fiber's microstructure. The effect is to increase the color saturation, richness, tightness, smoothness and flexibility of the fabric. And due to the violent shrinkage, the crystalline and non-crystalline areas inside the fiber are rearranged. This arrangement is more compact and orderly, producing a tightness that cannot be formed by weaving.

[0019] Preferably, the alkali shrinkage aid includes one or more of N-methylaminomethyl resin, urea-formaldehyde resin, melamine formaldehyde resin, isocyanate, and polyurethane.

[0020] Preferably, the concentration of the alkali shrinkage aid is 1-5% OWF.

[0021] In the textile field, OWF (On Weight of Fabric) means "fabric weight". When referring to the dosage of a chemical, using OWF means that the amount of the chemical added is calculated based on the dry weight of the fabric. OWF is a relative unit of measurement widely used in the textile industry. This method facilitates formula standardization and makes the production process more controllable and repeatable.

[0022] Although alkali shrinkage treatment can improve the performance of fabrics, the treatment process using high concentration alkali may cause the original strength of the fabric to decrease. In order to improve the dimensional stability of the fabric and make the fabric torsion-free, the present invention innovatively adds an alkali shrinkage aid with a cross-linking effect during the alkali shrinkage treatment process, which can effectively improve the dimensional stability and wrinkle resistance of the fabric. After the caustic soda treatment, the fiber surface is more open, which is conducive to the alkali shrinkage aid to better enter the fiber to form a cross-linked network, thereby enhancing the performance of the fabric.

[0023] Preferably, the subsequent dyeing and finishing process includes pre-treatment, cotton dyeing, post-treatment, color fixing, softening and shaping treatment of the fabric.

[0024] Preferably, the pretreatment comprises the following steps: placing the fabric in a dye vat at 10-40°C, adding a scouring agent to make its concentration in the dye bath 0.5-1.0 g / L, adding a lubricant to make its concentration in the dye bath 0.5-1.0 g / L, adding an alkali agent to make its concentration in the dye bath 1.0-1.5 g / L, adding a bleaching agent to make its concentration in the dye bath 1-5 g / L after running for 1-10 minutes, and the bath ratio is 1:(15-20); heating to 90-95°C, keeping the temperature for 45-60 minutes, then cooling to 60-70°C to drain, and then adding an acid solution to adjust the pH to 6-7.5; and then adding a deoxygenase to make its concentration in the dye bath 0.1-0.5 g / L.

[0025] Liquor Ratio refers to the ratio of the mass of the dyed fabric to the volume of the dye liquor used during the dyeing process. This is an important process parameter used to describe the amount of dye liquor relative to the fabric during the dyeing process. The choice of liquor ratio will affect the dyeing effect, cost and environmental factors.

[0026] In the pre-treatment step, preferably, the alkali agent is sodium hydroxide and the bleaching agent is hydrogen peroxide (H 2 O 2 ).

[0027] The acid solution used to adjust the pH mentioned herein includes one or more of acetic acid, citric acid, phosphoric acid, sulfuric acid, hydrochloric acid, formic acid, and carbonic acid. Acetic acid is more preferred. The concentration of the acid solution is preferably 0.1-1.0 g / L.

[0028] Preferably, the cotton dyeing comprises the following steps: adding an optimizer to 30-50°C water to make its concentration in the dye bath 0.1-1.0 g / L, running for 20-30 min, then adding a reactive dye and running for 10-20 min; adding Na 2 SO 4 Make its concentration in the dye bath 20~50g / L; add Na 2 CO 3The concentration of the dye in the dye bath is 10-30 g / L. After running for 5-30 minutes, the temperature is raised to 60-70°C at a rate of 0.1-1.0°C / min, and the liquid is discharged after keeping the temperature for 60-90 minutes.

[0029] In the cotton dyeing step, preferably, the optimizer is process optimizer AB-55.

[0030] In the cotton dyeing step, preferably, the reactive dyes include: 0.5-1.0% OWF yellow K-3RS, 0.01-0.1% OWF red K-3BS, and 0.3-0.5% OWF orange F-2R.

[0031] In the cotton dyeing step, preferably, Na is added twice. 2 SO 4 The specific operation is: first add 45~55wt%Na 2 SO 4 Run for 20-30 minutes, then add the remaining Na 2 SO 4 Run for 20 to 30 minutes.

[0032] In the cotton dyeing step, preferably, Na is added in batches. 2 CO 3 The specific operation is: first add 10~15wt%Na 2 CO 3 Run for 20-30 minutes, then add 20-25wt% Na 2 CO 3 Run for 20-30 minutes, then add 30-35wt% Na 2 CO 3 Run for 10-20 minutes, then add the remaining Na 2 CO 3 Run for 10 to 30 minutes.

[0033] Preferably, the post-treatment comprises the following steps: water inlet, adding 0.5-1.0% OWF acid solution, running for 5-10 minutes and then draining; water inlet, adding soaping agent so that its concentration in the dye bath is 1-5 g / L, heating to 95°C and keeping it warm for 10-30 minutes, then cooling to 60-70°C and draining; water inlet again, adding soaping agent so that its concentration in the dye bath is 1-5 g / L, heating to 95°C and keeping it warm for 10-30 minutes, then cooling to 60-70°C and draining; water inlet, heating to 75-85°C and keeping it warm for 10-30 minutes, then cooling to 60-70°C and draining.

[0034] Preferably, the color fixing and softening comprises the following steps: taking in water, adding 1-5% OWF softener and 1-5% OWF color fixing agent, running at 10-40°C for 10-30 minutes, adding silicone oil to make its concentration in the dye bath 1-5 g / L, adding acid solution to adjust the pH to 6-7.5, and running for 10-30 minutes before discharging the liquid out of the tank.

[0035] Preferably, the shaping comprises the following steps: placing the fabric in a shaping groove, adding a shaping aid in 20-60° C. water for shaping.

[0036] In the setting step, preferably, the setting aid comprises a softening oil and / or a smoothing agent, the concentration of the softening oil in the dye bath is 30-50 g / L, and the concentration of the smoothing agent in the dye bath is 20-40 g / L.

[0037] In the shaping step, preferably, the bath ratio during shaping is 1:(25-35).

[0038] In the shaping step, preferably, the shaping temperature is 150-180° C. and the shaping speed is 20-30 m / min.

[0039] Preferably, the production process further includes pre-shrinking and rolling packaging for warehousing after the fabric dyeing and finishing process.

[0040] The second object of the present invention is achieved by the following technical solutions:

[0041] A torsion-free plain woven fabric is produced by the above production process.

[0042] The torque test result of the non-torsion plain fabric can reach <0.5%.

[0043] Furthermore, after the plain weave fabric is knitted in a counterclockwise direction with a 32G needle density of a knitting machine and a yarn length of 10.5 cm / 50N, and is obtained by the alkali shrinkage process and subsequent dyeing and finishing process of the present invention, the torque test result can reach 0%.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] 1. The present invention provides a production process for a non-torsion plain weave fabric, which combines the optimal weaving process parameters with the innovative tension-free new alkali shrinkage treatment technology, so that the produced non-torsion plain weave fabric reaches an excellent level in terms of compactness. Under further optimal parameter settings, its torque test result is infinitely close to zero, and its performance is equivalent to that of traditional woven fabrics, and it can completely replace woven fabrics of the same thickness, showing excellent dimensional stability and non-torsion characteristics.

[0046] 2. The present invention provides a production process for a torsion-free plain fabric, which optimizes the weaving parameters during the weaving process, and ensures the uniformity and density of the fabric structure by accurately controlling the yarn twist, the tightness of the fabric, and the steering of the knitting machine. In the subsequent alkali shrinkage treatment stage, the tension-free alkali shrinkage treatment is used to effectively eliminate the stress accumulation of the fabric during the treatment process, thereby ensuring that the finished product has excellent dimensional stability and torsion-free characteristics.

[0047] 3. The present invention provides a production process for a torque-free plain weave fabric, which introduces an alkali shrinkage aid with a cross-linking effect during the alkali shrinkage treatment process, thereby significantly improving the dimensional stability of the fabric and ensuring its torque-free characteristics. Although the traditional alkali shrinkage treatment can improve the gloss and strength of the fabric, it still cannot guarantee the influence of the fabric on the torque after subsequent treatment. The present invention effectively overcomes this defect by adding an alkali shrinkage aid during the alkali shrinkage treatment, thereby achieving the torque-free characteristic of the fabric. The preferred alkali shrinkage aid of the present invention undergoes a cross-linking reaction with cellulose fibers under alkaline conditions to form a three-dimensional network structure, thereby enhancing the bonding force between the fibers and effectively reducing the torque phenomenon caused by uneven stress during the treatment of the fabric. This cross-linking effect also increases the dimensional stability of the fabric.

[0048] 4. The production process of a non-torsion plain fabric provided by the present invention not only significantly improves the quality of the plain fabric, but also greatly expands its application range, enabling it to replace traditional woven fabrics in more fields and meet the needs of different industries for high-quality and high-performance fabrics. Through this production process, we have successfully pushed the non-torsion plain fabric to a new technical level, ensuring that its performance in practical applications is more stable and reliable. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

[0050] Example 1

[0051] This embodiment provides a production process for a non-torsion plain weave fabric, and the production process comprises the following steps:

[0052] (1) Using a knitting machine to weave the yarn to obtain a blank cloth; the knitting machine specifications: diameter 34 inches, needle cylinder density 32G, total needle number 3000N, weaving in counterclockwise rotation; using a single-sided plain weave structure; the yarn length of the yarn is 10.5cm / 50N; the blank cloth piece weight: 20Kg / piece; after weaving is completed, the blank cloth is inspected and then enters the dyeing and finishing stage;

[0053] (2) The raw fabric was singed at a temperature of 1200°C and a speed of 90 m / min; then the raw fabric was immersed in a sodium hydroxide solution (30°C, 35°Bè) and 2.5% OWF N-methylaminomethyl resin was added for alkali shrinkage, so that the tensile tension of the raw fabric was 0, and the speed was 19 yards / min;

[0054] (3) Place the fabric in a dyeing vat at 25°C, add scouring agent HK-1031 (Ningbo Huake Auxiliary Agent Co., Ltd.) to make its concentration in the dye bath 1.0 g / L, add Yashihua LH-H (Ningbo Lianhua Chemical Co., Ltd.) to make its concentration in the dye bath 1.0 g / L, add NaOH to make its concentration in the dye bath 1.3 g / L, and add H after running for 5 minutes. 2 O 2 The concentration of the dye bath was 4g / L, and the bath ratio was 1:14. The temperature was raised to 95°C, kept for 45 minutes, and then cooled to 70°C to drain the solution. After draining, water was added again, and 0.8g / L acetic acid was added to adjust the pH to 7. Then, a deoxygenase was added to make the concentration in the dye bath 0.15g / L to remove H in the solution. 2 O 2 ;

[0055] (4) Add the new process optimizer AB-55 (Huntsman) to 40℃ water to make its concentration in the dye bath 0.5g / L. After running for 20 minutes, add the reactive dyes (Kyungin Co., Ltd., South Korea, 0.53% OWF Yellow K-3RS, 0.026% OWF Red K-3BS, 0.48% OWF Orange F-2R) and run for 10 minutes; add Na 2 SO 4 Make its concentration in the dye bath 35g / L (first add 50wt%Na 2 SO 4 Run for 30 min, then add the remaining 50 wt% Na 2 SO 4 Run for 20 min); add Na in batches 2 CO 3 Make its concentration in the dye bath 12g / L (first add 10wt% Na 2 CO 3 Run for 20 min, then add 20 wt% Na 2 CO3 Run for 20 min, then add 30 wt% Na 2 CO 3 Run for 10 min, then add the remaining 40 wt% Na 2 CO 3 Run for 10 minutes); then heat to 60°C at a rate of 0.5°C / min and keep warm for 60 minutes before draining;

[0056] (5) Inlet water, add 0.8% OWF acetic acid and run for 7 minutes before draining; Inlet water, add non-foaming soap detergent SW (BASF) to make its concentration in the dye bath 2g / L, heat to 90℃ and keep it warm for 10 minutes, then cool to 70℃ and drain; Inlet water, add non-foaming soap detergent SW (BASF) to make its concentration in the dye bath 2g / L, heat to 80℃ and keep it warm for 10 minutes, then cool to 70℃ and drain; Inlet water, heat to 80℃ and keep it warm for 10 minutes, then cool to 70℃ and drain;

[0057] (6) Add water, add 3% OWF anti-pinhole smoothing agent (Zhejiang Liansheng New Materials Co., Ltd.) and 2% OWF fixing agent G-200 (Ningbo Lianhua Chemical Co., Ltd.), run at 25°C for 10 minutes, add silicone oil 102 (Jiangmen Green Textile Technology Co., Ltd.) to make its concentration in the dye bath 1-5 g / L, add 0.15 g / L acetic acid to adjust the pH to 7, run for 10 minutes, and drain the liquid out of the tank;

[0058] (7) Place the fabric in a setting trough, add soft oil (Shaoxing Demei New Materials Co., Ltd.) to 50°C water to make its concentration in the dye bath 40g / L, add smoothing agent SF-14 (Ningbo Lianhua Co., Ltd.) to make its concentration in the dye bath 30g / L, the bath ratio is 1:30, the setting temperature is 160°C, and the setting speed is 28m / min;

[0059] (8) Finally, the torsion-free plain fabric product is obtained after pre-shrinking, rolling and packaging for storage.

[0060] Comparative Example 1

[0061] The difference between this comparative example and Example 1 is that the yarn length used is 11.5 cm / 50N, and the rest is the same as Example 1.

[0062] Comparative Example 2

[0063] The difference between this comparative example and Example 1 is that the yarn length used is 12cm / 50N, and the rest is the same as Example 1.

[0064] Comparative Example 3

[0065] The difference between this comparative example and Example 1 is that the yarn length used is 13cm / 50N, and the rest is the same as Example 1.

[0066] Comparative Example 4

[0067] The difference between this comparative example and embodiment 1 is that the knitting machine rotates clockwise for weaving, and the rest is the same as embodiment 1.

[0068] Comparative Example 5

[0069] The difference between this comparative example and Example 1 is that the needle cylinder density of the knitting machine is 28G, and the rest is the same as Example 1.

[0070] Comparative Example 6

[0071] The difference between this comparative example and Example 1 is that no alkali shrinkage treatment is performed, and the rest is the same as Example 1.

[0072] Comparative Example 7

[0073] The difference between this comparative example and Example 1 is that no alkali shrinkage aid is added during the alkali shrinkage treatment, and the rest is the same as Example 1.

[0074] The above embodiments and comparative examples were used to test the twist rate of the fabric according to the method of GB / T23319.3.1. The specific parameter settings and test results are shown in Table 1.

[0075] Table 1 Fabric parameter settings and torque test results of the embodiment and the comparative example

[0076] As shown in Table 1, it can be seen from Example 1 that the plain fabric obtained by the production process of the technical solution of the present invention has achieved an excellent level in eliminating torque, and its tightness has almost reached the extreme. The torque test result of the product fabric is infinitely close to zero, which is the same as that of woven fabrics, and can completely replace woven fabrics of the same thickness; while the plain fabrics obtained by the production process of the technical solution of the present invention in Comparative Examples 1 to 7 have different degrees of increase in the torque test results, and cannot reach the level of no torque in the embodiment.

[0077] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0078] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0079] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A production process for a non-torsion plain weave fabric, characterized in that: The production process comprises the following steps: using a knitting machine to weave yarn to obtain a blank cloth; subjecting the blank cloth to an alkali shrinkage treatment, and then to a subsequent dyeing and finishing process to obtain a finished product of a torsion-free plain weave cloth; The knitting machine includes the following parameters: diameter of 30-50 inches, needle density of 30-50G, total needle number of 2500-5000N, weaving in counterclockwise rotation; yarn length of the yarn is 9-11cm / 50N; the weaving structure is the structure of single-sided plain cloth; The alkali shrinkage treatment comprises: immersing the raw cloth in an alkali agent and adding an alkali shrinkage auxiliary agent to perform alkali shrinkage treatment, so that the tensile tension of the raw cloth is 0 and the treatment speed is 10-30 yards / min; The alkali shrinkage aid includes one or more of N-methylaminomethyl resin, urea-formaldehyde resin, melamine formaldehyde resin, isocyanate, and polyurethane.

2. The production process of a non-torsion plain fabric according to claim 1, characterized in that: The concentration of the alkali shrinkage aid is 1-5% OWF.

3. The production process of a non-torsion plain fabric according to claim 1, characterized in that: The alkali agent is a sodium hydroxide solution, the temperature of the alkali agent is 25-35°C, and the concentration is 25-45°Bè.

4. The production process of a non-torsion plain fabric according to claim 1, characterized in that: After the weaving is completed, the blank cloth needs to be singed, and the burner temperature during the singeing process is 1100-1200° C. and the speed is 80-95 m / min.

5. The production process of a non-torsion plain fabric according to claim 1, characterized in that: The subsequent dyeing and finishing process includes pre-treatment, cotton dyeing, post-treatment, color fixing, softening and shaping treatment of the fabric.

6. The production process of a non-torsion plain fabric according to claim 5, characterized in that: The pretreatment comprises the following steps: placing the fabric in a dyeing vat at 10-40°C, adding a scouring agent to make its concentration in the dyeing bath 0.5-1.0 g / L, adding a lubricant to make its concentration in the dyeing bath 0.5-1.0 g / L, adding an alkali agent to make its concentration in the dyeing bath 1.0-1.5 g / L, adding a bleaching agent to make its concentration in the dyeing bath 1-5 g / L after running for 1-10 minutes, and the bath ratio is 1:(15-20); heating to 90-95°C, keeping the temperature for 45-60 minutes, then cooling to 60-70°C to drain, and then adding an acid solution to adjust the pH to 6-7.5; and then adding a deoxygenase to make its concentration in the dyeing bath 0.1-0.5 g / L.

7. The production process of a non-torsion plain fabric according to claim 5, characterized in that: The cotton dyeing method comprises the following steps: adding an optimizer to water at 30-50°C to make its concentration in the dye bath 0.1-1.0 g / L, running for 20-30 minutes, adding a reactive dye and running for 10-20 minutes; adding Na2SO4 and making its concentration in the dye bath 20-50 g / L; adding Na2CO3 and making its concentration in the dye bath 10-30 g / L; running for 5-30 minutes, heating to 60-70°C at a rate of 0.1-1.0°C / min, keeping the temperature for 60-90 minutes and then draining.

8. The production process of a non-torsion plain fabric according to claim 5, characterized in that: The color fixing and softening process comprises the following steps: adding water, adding 1-5% OWF softener and 1-5% OWF color fixing agent, running at 10-40° C. for 10-30 minutes, adding silicone oil to make its concentration in the dye bath 1-5 g / L, adding acid solution to adjust the pH to 6-7.5, and running for 10-30 minutes before discharging the liquid out of the tank.

9. The production process of a non-torsion plain fabric according to claim 5, characterized in that: The shaping process comprises the following steps: placing the fabric in a shaping groove, adding a shaping aid to water at 20-60°C for shaping; the shaping aid comprises a softening oil and / or a smoothing agent, the concentration of the softening oil in the dye bath is 30-50 g / L, and the concentration of the smoothing agent in the dye bath is 20-40 g / L; the bath ratio during shaping is 1:(25-35); the shaping temperature is 150-180°C, and the shaping speed is 20-30 m / min.

10. A non-torsion plain fabric, characterized in that: The method is produced by the production process according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Energy-saving dyeing and finishing method for thin cotton spandex knitted fabric

    CN111733590A

  • Dyeing and finishing process of knitted cotton fabric with cool and thick hand feeling and product thereof

    CN114875597A

  • Processing method of pure linen yarn pretreatment process

    CN116200943A

  • Method and appts. for eliminating spirality in knitted fabric

    CN1222206A

  • Method for eliminating straight line skew of one-side weft-knitted fabric

    CN1546770A