ScAlMgO4 single crystal substrate and manufacturing method thereof

By controlling the oxygen concentration and atmosphere conditions of the ScAlMgO4 single crystal substrate, the warping and cracking of GaN film during growth on the ScAlMgO4 substrate is solved, the cleavage of the substrate and the stability of the film are improved, and the ScAlMgO4 single crystal substrate is realized. Effects of growing high brightness GaN films.

CN111560648BActive Publication Date: 2024-11-12PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010082054.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-14
Filing Date
2020-02-06
Publication Date
2024-11-12
Estimated Expiration
2040-02-06

AI Technical Summary

Technical Problem

When the GaN film is grown on the ScAlMgO4 single crystal substrate, warping and rupture are prone to occur, resulting in increased stress on the film, and thus rupture of the film.

Method used

During the manufacturing process of ScAlMgO4 single crystal substrate, the oxygen concentration in the crystal is controlled to be less than 57 atomic % and crystal lift is performed in a low oxygen atmosphere (0.1 volume % or less), and high-frequency heating or resistance heating is used to perform crystal lifting. , adjust the temperature gradient directly below the liquid level of the melt to reduce the oxygen concentration and increase the temperature gradient, reduce the dissolution of oxygen into the melt, thereby improving the cleavage of the substrate.

Benefits of technology

It is realized that the GaN film is not prone to cracking when growing on the ScAlMgO4 single crystal substrate, which improves the cleavage of the substrate and the stability of the film, and avoids the rupture of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111560648B_ABST
    Figure CN111560648B_ABST
Patent Text Reader

Abstract

The present invention provides a ScAlMgO4 single crystal substrate having high cleavage and a GaN film grown on the substrate that is not easily cracked, and a method for manufacturing the same. The oxygen concentration in the crystal analyzed by inductively coupled plasma emission spectrometry is set to 57 atomic % or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a ScAlMgO4 single crystal substrate and a method for manufacturing the same. Background Art

[0002] In recent years, ScAlMgO4 has attracted attention as a substrate for forming gallium nitride (GaN). The lattice mismatch between ScAlMgO4 and GaN is only 1 / 10 of that of conventional sapphire, making it a promising material for achieving higher brightness of light-emitting diodes (LEDs).

[0003] As a method for manufacturing ScAlMgO4 single crystal, the Czochralski method (CZ method) is known. In the CZ method, a material is placed in a crucible set in a chamber, and after the material is melted, a seed crystal is brought into contact with the melt. In addition, a pulling mechanism is used to slowly rotate the seed crystal while pulling it, thereby growing a single crystal with the same orientation arrangement as the seed crystal, and obtaining a cylindrical ingot.

[0004] Patent Documents 1 and 2 describe methods for producing ScAlMgO 4 .

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-48296

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-178448 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, when a GaN film is grown on a ScAlMgO 4 single crystal substrate, there is a problem that the GaN film and the ScAlMgO 4 single crystal substrate are warped, and thus stress is applied to each other, causing the GaN film to crack.

[0011] The purpose of the present application is to solve the above-mentioned problems and to provide a ScAlMgO4 single crystal substrate in which the grown GaN film is less likely to crack and a method for manufacturing the same.

[0012] Means for solving problems

[0013] In the ScAlMgO4 single crystal substrate of the present application, the oxygen concentration in the crystal analyzed by inductively coupled plasma emission spectrometry is set to 57 atomic % or less.

[0014] In addition, the manufacturing method of the ScAlMgO4 single crystal substrate of the present application comprises the following steps: a seeding step of bringing a seed crystal into contact with a raw material melt of the single crystal substrate represented by ScAlMgO4 to generate a crystal; and a crystal growing step of pulling the crystal generated by the seeding step to grow a single crystal. In the crystal growing step, the crystal is pulled from the melt in an atmosphere with an oxygen concentration of 0.1 volume % or less.

[0015] Effects of the Invention

[0016] According to the present application, it is possible to provide a ScAlMgO4 single crystal substrate having high cleavage resistance and a GaN film grown on the substrate that is not easily cracked, and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic diagram showing the structure of a high-frequency heating furnace used in a method for manufacturing a ScAlMgO4 single crystal substrate according to an embodiment of the present application.

[0018] Figure 2 This is a flow chart for manufacturing a single crystal by a method for manufacturing a ScAlMgO4 single crystal substrate according to one embodiment of the present application.

[0019] Figure 3 This is a schematic diagram showing the structure of a resistance heating furnace used in a method for manufacturing a ScAlMgO4 single crystal substrate according to an embodiment of the present application.

[0020] Figure 4 This is a diagram showing the crystal structure of a ScAlMgO4 single crystal substrate according to one embodiment of the present application observed using a transmission electron microscope.

[0021] Description of Reference Numerals

[0022] 100 High frequency heating furnace

[0023] 110 ScAlMgO4 raw material

[0024] 120 Crucible

[0025] 121 Crucible support shaft

[0026] 122 Refractory materials

[0027] 130 Insulation Materials

[0028] 140 Heating coil

[0029] 150 Crystallization pull shaft

[0030] 151 Seed Holder

[0031] 152 Seed

[0032] 300 Resistance Heating Furnace

[0033] 330 Insulation Materials

[0034] 340 Heater DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0036] (Implementation Method)

[0037] Figure 1 This is a schematic diagram showing the structure of a high-frequency heating furnace used in a method for manufacturing a ScAlMgO4 single crystal substrate according to an embodiment of the present application. The following mainly describes the case of manufacturing a ScAlMgO4 single crystal substrate by a high-frequency heating method. Among them, a resistance heating method can also be used instead of the high-frequency heating method. According to the method of this embodiment, a ScAlMgO4 single crystal substrate with a low oxygen concentration in the crystal (specifically, the oxygen concentration in the crystal obtained by analyzing using an inductively coupled plasma emission spectrometry method is less than 57 atomic %) can be obtained. This ScAlMgO4 single crystal substrate has a high cleavage property. Therefore, when a GaN film is grown on a ScAlMgO4 single crystal substrate, the GaN film can be prevented from breaking.

[0038] Figure 1 The high frequency heating furnace 100 shown is a crystal pulling device based on the CZ method, and comprises a raw material 110 of a ScAlMgO4 single crystal substrate, a crucible 120, a crucible support shaft 121, a refractory material 122, a heat insulating material 130, a heating coil 140, a crystal pulling shaft 150, a seed crystal holder 151 and a seed crystal 152. It should be noted that although Figure 1 Although not shown, the high-frequency heating furnace 100 generally includes a chamber, a vacuum pump, a gas inlet, a gas outlet, a power source, a temperature control device, and the like necessary for crystal pulling based on the CZ method.

[0039] In this embodiment, the raw material of the ScAlMgO4 single crystal substrate (hereinafter also referred to as "ScAlMgO4 raw material") 110 is a material obtained by mixing scandium oxide (Sc2O3), aluminum oxide (Al2O3) and magnesium oxide (MgO) in a specified ratio and melting them once.

[0040] In this embodiment, the crucible 120 is made of iridium and is a container for holding the ScAlMgO4 raw material 110. In addition, in this embodiment, the crucible support shaft 121 is made of tungsten and is a shaft for supporting the crucible 120. The crucible support shaft 121 can rotate or lift the crucible 120 at a set speed.

[0041] The refractory material 122 is a member disposed between the crucible 120 and the crucible support shaft 121. In the present embodiment, the refractory material 122 is made of zirconia, but is not limited thereto. The refractory material 122 has a reactivity resistance to any material of the crucible 120 and the crucible support shaft 121.

[0042] In addition, the heat insulating material 130 is made of zirconium oxide in this embodiment. The heat insulating material 130 surrounds the crucible 120, and has a through hole for inserting the crystal pulling shaft 150 and a through hole for inserting the crucible support shaft 121 at the upper and lower parts of the crucible 120, respectively. In addition, the heating coil 140 is arranged on the outside of the heat insulating material 130. When a high-frequency current flows through the heating coil 140, a high-frequency magnetic flux is generated. In addition, due to the high-frequency magnetic flux, an eddy current is generated in the crucible 120, and the surface of the crucible 120 is heated, thereby heating the ScAlMgO4 raw material 110 in the crucible 120.

[0043] The crystal pulling shaft 150 of this embodiment is made of alumina and has the function of rotating and lifting at a set speed. The seed holder 151 is arranged at the front end of the crystal pulling shaft 150. In this embodiment, the seed holder 151 is made of iridium, and a seed 152 can be set at the front end. In addition, the seed 152 set in the seed holder 151 is ScAlMgO4, and the shape is a regular quadrangular prism, but it is not limited to this shape.

[0044] Regarding the case of manufacturing ScAlMgO4 single crystal using the high frequency heating furnace 100, the Figure 2 The flowchart shown is used for explanation.

[0045] First, a melting process (S201) is performed to melt the ScAlMgO4 raw material 110. In the melting process, in order to make the atmosphere in the high-frequency heating furnace 100 an inert gas atmosphere, vacuum is performed. Then, an inert gas atmosphere is introduced and set to normal pressure. After the power is turned on, the power applied to the heating coil 140 is gradually increased over a period of time to heat the crucible 120 to a degree that does not impose a large load on the crucible 120 until the temperature at which the ScAlMgO4 raw material 110 melts is reached. The heating time depends on the size of the crucible 120. When the outer diameter of the crucible 120 is 80 mm to 150 mm, it is preferably 15 hours to 60 hours.

[0046] After confirming that the ScAlMgO4 raw material 110 is melted, oxygen is introduced into the furnace. It should be noted that the concentration of oxygen can be adjusted by the ratio of the introduced inert gas and oxygen. For example, when the inert gas is nitrogen and its gas introduction amount is 1 [1 / min], when the gas flow rate of the mixed oxygen is set to 1 [ml / min], the oxygen concentration in the atmosphere in the furnace becomes 0.1 volume %. Similarly, when the inert gas is nitrogen and its gas introduction flow rate is 2 [1 / min], when the mixed oxygen gas flow rate is set to 10 [ml / min], the oxygen concentration in the atmosphere in the furnace becomes 0.5 volume %. In this embodiment, it is preferably set to be in an atmosphere with an oxygen concentration of less than 0.1 volume %, and the seeding step (S202) and crystal growth step (S203) described later are performed. And in particular, 0 volume % < oxygen concentration is more preferably.

[0047] Next, the seeding step (S202) is performed. Specifically, the crystal pulling shaft 150 is rotated at a predetermined speed while slowly descending until the seed crystal 152 contacts the molten ScAlMgO4 raw material 110. After the seed crystal 152 contacts the molten ScAlMgO4 raw material 110, wait until the melt temperature of the molten ScAlMgO4 raw material 110 stabilizes at a temperature suitable for crystal pulling.

[0048] Next, the crystal generated by the seeding step (202) is pulled, thereby implementing a crystal growing step (S203) of growing a single crystal. The crystal pulling shaft 150 is rotated at a specified speed while rising at a specified speed. Here, it is preferred that the rotation speed of the crystal pulling shaft 150 is 1rpm to 10rpm, and the pulling speed is 0.1mm / hour to 1.5mm / hour. After the pulling starts, the automatic diameter control (Automatic Diameter Control (ADC)) is used to control the desired crystal shape. After the crystal is pulled to the desired length, the crystal is separated from the melt of the molten ScAlMgO4 raw material 110, and the introduction of oxygen into the furnace is stopped.

[0049] Next, a cooling step (S204) is performed. The power applied to the heating coil 140 is slowly reduced over time to cool the crucible 120 and the pulled crystal without applying a large load. The cooling time depends on the size of the crucible 120. When the outer diameter of the crucible 120 is 80 mm to 150 mm, it is preferably 20 hours to 70 hours.

[0050] On the other hand, Figure 3As shown, the resistance heating furnace 300 that can be used in the manufacturing method of the ScAlMgO4 single crystal substrate of this embodiment is different from the high-frequency heating furnace 100 in that it has a heat insulating material 330 and a heater 340 instead of the heat insulating material 130 and the heating coil 140, and other aspects can be set to be the same as the high-frequency heating furnace 100.

[0051] In the resistance heating furnace 300, the heat insulating material 330 is made of carbon and is arranged to surround the crucible 120. In addition, the heater 340 is made of carbon in a cylindrical shape, and when current flows through the heater 340, the heater 340 generates heat, and the ScAlMgO4 raw material 110 in the crucible 120 is heated.

[0052] When the ScAlMgO4 single crystal is produced by the resistance heating furnace 300, the heating temperature can be set to Figure 2 The manufacturing process shown. First, a melting process (S201) of the ScAlMgO4 raw material 110 is implemented. The melting process can be set to the same as the case of using the above-mentioned high-frequency heating furnace 100. For example, in the melting process, in order to make the atmosphere an inert gas atmosphere, after evacuation, the inert gas atmosphere is set to normal pressure. And, after the power is turned on, the power applied to the heater 340 is gradually increased over a period of time to heat the crucible 120 to a degree that does not impose a large load on the crucible 120 until the temperature at which the ScAlMgO4 raw material 110 melts is reached. The heating time is the same as the case of using the high-frequency heating furnace 100, and in this case, the oxygen concentration in the furnace is also adjusted by the ratio of the introduced inert gas and oxygen.

[0053] Next, a seeding step ( S202 ), a crystal growth step ( S203 ), and a cooling step ( S204 ) are performed. These steps can be performed in the same manner as in the case of using the high-frequency heating furnace 100 described above.

[0054] By adjusting the oxygen concentration in the atmosphere in which the crystal growth step (S203) is performed to 0.1% by volume or less when manufacturing the ScAlMgO4 single crystal substrate using either the high-frequency heating furnace 100 or the resistance heating furnace 300, it is easy to obtain a ScAlMgO4 single crystal substrate having an oxygen concentration of 57 atomic % or less in the crystal analyzed by inductively coupled plasma emission spectrometry and having a high cleavage resistance. In particular, by adjusting the temperature gradient just below the liquid surface of the melt of the ScAlMgO4 raw material 110 in the crystal growth step (S203), it is easy to obtain a ScAlMgO4 single crystal substrate with a higher cleavage resistance.

[0055] Specifically, when the oxygen concentration in the furnace atmosphere is reduced and the temperature gradient just below the liquid surface of the melt of the melted ScAlMgO4 raw material 110 is increased (the temperature decreases for every 1 mm increase in the distance from the melt surface), the amount of oxygen dissolved in the melt is suppressed, and the oxygen concentration in the pulled crystal is reduced. In order to increase the temperature gradient just below the liquid surface of the melt, it is necessary to increase the difference between the maximum temperature and the minimum temperature on the side of the crucible 120. When the maximum temperature on the side of the crucible 120 increases, an area where the melt temperature becomes high is generated, and when the melt is an oxide, oxygen is removed from the melt. And at this time, if the oxygen concentration in the furnace atmosphere is low, the oxygen concentration in the pulled crystal is reduced.

[0056] However, if the maximum temperature of the side of the crucible 120 increases, the convection of the melt in the crucible 120 intensifies. As a result, in the seeding step (S202), the melt temperature of the molten ScAlMgO4 raw material 110 is not easy to stabilize. Therefore, it is preferred to control the temperature of the melt with an accuracy of 0.5 [°C] or less to achieve stabilization at a temperature suitable for crystal pulling.

[0057] Figure 4 The ScAlMgO4 single crystal substrate produced by the above method is observed by a transmission electron microscope. The ScAlMgO4 single crystal has a ScO2 layer ( Figure 4 Sc layer) and the hexagonal AlMgO2 layer ( Figure 4 The ScAlMgO4 single crystal is cleaved between the AlMgO2 layers with weak bonding strength. Furthermore, if the oxygen concentration in the crystal is reduced, the oxygen bonds between the AlMgO2 layers with weak bonding strength decrease, and the cleavage is further improved.

[0058] Here, for the temperature gradient just below the liquid surface of the melt of the melted ScAlMgO4 raw material 110, if the opening area of ​​the through hole for inserting the crystallization pulling shaft 150 on the upper part of the heat insulating material 130 or 330 is changed in any of the high-frequency heating furnace 100 and the resistance heating furnace 300, the temperature gradient also changes. If the opening area of ​​the through hole becomes wider, the temperature gradient becomes smaller, and if the opening area becomes narrower, the temperature gradient becomes larger. That is, as described in detail later, by manufacturing the ScAlMgO4 single crystal substrate in a manner such that the temperature gradient just below the liquid surface of the melt is 4.4°C / mm or more, it is possible to manufacture a ScAlMgO4 single crystal with a lower oxygen concentration.

[0059] The substrate of the desired thickness is cut from the pulled ScAlMgO4 single crystal by processing methods such as cleavage, laser slicing, and wire slicing to produce a ScAlMgO4 single crystal substrate. The front and back surfaces of the ScAlMgO4 single crystal substrate become the main surfaces, which are used as the surfaces for growing GaN films, etc. The main surfaces can also be mirror-finished by grinding, grinding, etc.

[0060] It should be noted that, in the present embodiment, when the ScAlMgO4 single crystal substrate is used as a growth substrate for various films (e.g., GaN films), it is preferred to set the radius of curvature R [m] of the ScAlMgO4 single crystal substrate and the thickness t of the ScAlMgO4 single crystal substrate in such a manner that σ in the following formula satisfies 5.0 or more. s [m].

[0061] σ[N / mm 2 ]≤(E f ×t f 2 )×10 3 / (6×(1-v f )×R×t s )

[0062] (In the above formula, E f [GPa] represents the Young's modulus of the film (here, GaN film) grown on the crystalline ScAlMgO4 single crystal substrate, v f represents the Poisson's ratio of the film to be crystallized (GaN film in this case), t f [m] represents the thickness of the film to be crystal-grown (here, the GaN film)

[0063] As described in detail in the embodiment, when the radius of curvature R [m] and the thickness ts [m] of the ScAlMgO4 single crystal substrate are adjusted to satisfy the above formula, the stress (warping stress) generated when various films (here, GaN film) are grown on the ScAlMgO4 single crystal substrate exceeds the cleavage strength of the ScAlMgO4 single crystal substrate. Therefore, before the film (GaN film) grown by the warping stress is broken, the ScAlMgO4 single crystal substrate is cleaved and peeled off from the film (GaN film) grown by the warping stress.

[0064] It should be noted that, regarding the ScAlMgO4 single crystal substrate, it is preferred that the full width at half maximum (seconds) of the rocking curve obtained by analyzing the sliced ​​wafer by X-ray diffraction method be 20 (seconds) or less.

[0065] When a GaN film is formed on a ScAlMgO4 single crystal substrate, the GaN film is formed by a so-called vapor phase growth method such as a hydride vapor phase epitaxy method (HVPE method) or a metal organic chemical vapor phase growth method (MOCVD method). On the other hand, a GaN film can also be formed by a liquid phase growth method such as a flux method using an alkali metal melt (flux) represented by a sodium flux method.

[0066] It should be noted that in the above description, the heat insulating materials 130 and 330 are made of zirconia, but are not limited thereto. The crucible 120 and the seed crystal holder 151 are made of iridium, but are not limited thereto. The crucible support shaft 121 is made of tungsten, but is not particularly limited as long as it does not react with the refractory material 122. The refractory material 122 is made of zirconia, but is not particularly limited as long as it does not react with the crucible 120 and the crucible support shaft 121. The crystal pulling shaft 150 is made of alumina, but is not particularly limited as long as it does not react with the seed crystal holder 151.

[0067] Example

[0068] [Examples 1, 2 and Comparative Example 1]

[0069] Will use Figure 1 The results of growing a GaN film on a ScAlMgO4 single crystal substrate by using the high frequency heating furnace 100 shown in Table 1 are shown in Table 1. In Comparative Example 1 and Examples 1 and 2, the oxygen concentration of the atmosphere in the furnace (crystal growing process) and the temperature gradient just below the liquid surface of the melt are changed as shown in Table 1. In addition, Table 1 also shows the oxygen concentration in the obtained ScAlMgO4 single crystal substrate, the cleavage strength of the pulled crystal, whether the ScAlMgO4 single crystal substrate is peeled off when the GaN film is grown on the ScAlMgO4 single crystal substrate, and whether the GaN film is cracked.

[0070] It should be noted that the oxygen concentration in the atmosphere of the high-frequency heating furnace 100 (especially the crystal growth process) is adjusted in the furnace by the flow rate of the inert gas (nitrogen) and the flow rate of oxygen. In Examples 1 and 2, the flow rate of the mixed oxygen is set to 1 [ml / min] relative to the flow rate of the inert gas (nitrogen) of 1 [1 / min]. In Comparative Example 1, the flow rate of the mixed oxygen is set to 5 [ml / min] relative to the flow rate of the inert gas (nitrogen) of 1 [1 / min]. It should be noted that, although not shown in Table 1, when the oxygen amount is set to 0, the surface of the crystal is colored white and cracks are generated. This is because the oxygen concentration in the crystal becomes too small.

[0071] In addition, the temperature gradient just below the liquid surface of the molten liquid is adjusted by the opening area of ​​the through hole for inserting the crystal pulling shaft 150. Specifically, when the opening area of ​​the through hole in Comparative Example 1 is set to 1.00, it is set to 0.41 in Example 1. As a result, the temperature gradient just below the liquid surface of the molten liquid becomes 4.7°C / mm. In addition, the opening area is set to 0.56 in Example 2. As a result, the temperature gradient just below the liquid surface of the molten liquid becomes 4.4°C / mm.

[0072] [Measurement and evaluation of physical properties]

[0073] The measurement and evaluation of each numerical value were performed by the following method.

[0074] Oxygen concentration in crystals

[0075] The oxygen concentration in the crystal was measured using inductively coupled plasma emission spectrometry. Specifically, iCAP 7400Duo (manufactured by Thermo Fisher Scientific) was used as an inductively coupled plasma emission spectrometry analyzer to analyze Sc, Al, and Mg, which are the main components of the ScAlMgO4 single crystal. O was calculated by subtracting the analytical values ​​of Sc, Al, and Mg and taking all the remainder as O.

[0076] ·Temperature gradient just below the melt surface

[0077] Regarding the temperature gradient just below the melt surface, a tungsten (W)-rhenium (Re) thermocouple (W·5%Re-W·26%Re) was inserted into an iridium protection tube. Figure 1 The through hole of the crystal pulling shaft 150 of the heat insulating material 130 is used, and the iridium protection tube is lowered instead of the crystal pulling shaft 150 to make it touch the molten ScAlMgO4 raw material 110 in the crucible 120 for measurement.

[0078] Cleavage strength

[0079] The cleavage strength was measured by using a small tabletop tester EX-S500N (manufactured by Shimadzu Corporation) to bond an aluminum rivet to a ScAlMgO4 single crystal substrate. The bonded aluminum rivet was stretched to measure the force when the ScAlMgO4 single crystal substrate was cleaved and peeled off.

[0080] ·Substrate peeling and growth film rupture

[0081] The peeling of the substrate and the breakage of the grown film were confirmed visually.

[0082] [Table 1]

[0083] Example 1 Example 2 Comparative Example 1 Oxygen concentration in atmosphere [volume %] 0.1 0.1 0.5 Temperature gradient just below the melt surface [℃ / mm] 4.7 4.4 2.6 <![CDATA[Cleavage strength [N / mm 2 > 4.9 5.0 8.2 Oxygen concentration in crystal [atomic %] 56 57 58 Substrate peeling have have none Rupture of the growing film none none have

[0084] From Table 1, it can be understood that if the oxygen concentration in the atmosphere during the crystal growth process is set to 0.1 volume % or less, and the temperature gradient just below the melt surface is set to 4.4°C / mm or more, the oxygen concentration in the resulting crystal is reduced, and the cleavage strength is reduced. In addition, if the oxygen concentration in the crystal is 57 atomic % or less, the cleavage strength becomes 5.0 N / mm 2 Furthermore, in this case, when a GaN crystal is grown on the ScAlMgO4 single crystal substrate, even if stress is applied, the ScAlMgO4 single crystal substrate is peeled off before the GaN film is broken, and the GaN film grown on the substrate is not broken.

[0085] [About stress applied to ScAlMgO4 single crystal substrate]

[0086] The stress applied to the ScAlMgO4 single crystal substrate when GaN crystal is grown on the main surface of the ScAlMgO4 single crystal substrate is described. The stress σ [N / mm 2 ] is expressed by the Stoney formula (Formula 1). Here, E f [GPa] is the Young's modulus of the growing film, v f is the Poisson's ratio of the growing film, t f [m] is the thickness of the growing film, t s [m] is the thickness of the ScAlMgO4 single crystal substrate, and R[m] is the radius of curvature of the grown film.

[0087] σ=(E f ×t f 2 )×10 3 / (6×(1-v f )×R×t s )···(Formula 1)

[0088] When the grown film is a GaN film, Young's modulus E f is 321GPa, Poisson's ratio v f For example, when the thickness of the GaN film is 1 mm, when the thickness of the ScAlMgO4 single crystal substrate is changed, the stress applied to the ScAlMgO4 single crystal substrate becomes 5.0 N / mm 2 The range of the above curvature radius R [m] is shown in Table 2. R in Formula 1 is originally the curvature radius of the growth film, but the growth film is grown on the ScAlMgO4 single crystal substrate, so their curvature radii are the same. It should be noted that from the perspective of reliability, it is preferred to set σ less than 8.2 [N / mm 2] to set the radius of curvature R [m] of the ScAlMgO4 single crystal substrate and the thickness t of the ScAlMgO4 single crystal substrate s [m].

[0089] [Table 2]

[0090] GaN film thickness [mm] <![CDATA[Thickness of the scAlMgO4 single crystal substrate [μm]]]> Range of curvature radius [m] 1 400 Under 33 1 300 Below 44 1.5 400 Below 75 1.5 300 Below 100

[0091] As described above, the thickness of the GaN film to be grown is set to 1 mm or 1.5 mm, but the GaN film can be set to a desired value. In this case, as long as the oxygen concentration of the ScAlMgO4 single crystal substrate is controlled to be less than 57 atomic %, and the thickness t of the desired GaN film is selected, f The curvature radius R and the thickness t of the ScAlMgO4 single crystal substrate satisfy 5.0≤σ s The ScAlMgO4 single crystal substrate can be manufactured. f If the GaN film is warped, the stress applied to the ScAlMgO4 single crystal substrate exceeds the cleavage strength of the ScAlMgO4 single crystal substrate. Therefore, before the GaN film breaks, the ScAlMgO4 single crystal substrate can be peeled off and the internal stress can be released.

[0092] It should be noted that the curvature radius R of the ScAlMgO4 single crystal substrate s [m] varies according to the rotation speed a [rpm] and the pulling speed b [mm / h] of the crystal pulling shaft 150. The curvature radius R of the ScAlMgO4 single crystal substrate is set to the same conditions as Example 1 in Table 1 except for the rotation speed a [rpm] and the pulling speed b [mm / h]. s [m] is shown in Table 3.

[0093] [Table 3]

[0094] Speed ​​a[rpm] Pulling speed b[mm / h] <![CDATA[Radius of curvature R of ScAlMgO4 single crystal substrate s [m]]]> 5 0.7 30.0 2 0.7 129.9 5 0.3 15.8

[0095] It can be seen from Table 3 that if the rotation speed a[rpm] is reduced, the curvature radius R of the ScAlMgO4 single crystal substrate s [m] becomes larger. If the pulling speed b[mm / h] is reduced, the curvature radius R of the ScAlMgO4 single crystal substrate s [m] becomes smaller.

[0096] According to the ScAlMgO4 single crystal substrate of the present application, the cleavage of the ScAlMgO4 single crystal substrate can be improved. As a result, the cracking of the GaN film grown on the substrate can be suppressed. It should be noted that the film grown on the ScAlMgO4 single crystal substrate is preferably GaN, but the material satisfying σ of 5.0 or more in Formula 1 can also be suitable for use as a growth film.

[0097] Industrial Applicability

[0098] The ScAlMgO4 single crystal substrate and the method for manufacturing the same of the present invention can be used for forming GaN films, etc.

Claims

1. A ScAlMgO4 single crystal substrate, wherein: The oxygen concentration in the crystal analyzed by inductively coupled plasma emission spectrometry is 56 atomic % or more and 57 atomic % or less. Cleavage strength is 5.0N / mm 2 the following.

2. The ScAlMgO4 single crystal substrate according to claim 1, which is a substrate for crystal growth and has a value of σ in the following formula satisfying 5.0 N / mm 2 The radius of curvature R and thickness t s , σ=(E f ×t f 2 )×10 3 / (6×(1-v f )×R×t s ) In the above formula, E f represents the Young's modulus of the film to be crystallized, v f represents the Poisson's ratio of the film to be crystallized, t f represents the thickness of the film to be grown. in, The unit of R is m, t s The unit is m, E f The unit is GPa, t f The unit is m.

3. The ScAlMgO4 single crystal substrate according to claim 2, wherein: The film to be crystal-grown is GaN.

4. A method for manufacturing a ScAlMgO4 single crystal substrate, which is the method for manufacturing a ScAlMgO4 single crystal substrate according to claim 1 or 2, comprising the following steps: A seeding step of bringing a seed crystal into contact with a raw material melt of a single crystal substrate represented by ScAlMgO4 to generate a crystal; and a crystal growing step of pulling up the crystal generated by the seeding step to grow a single crystal, In the crystal growing step, the crystal is pulled from the melt in an atmosphere having an oxygen concentration of 0.1% by volume or less.

5. The method for manufacturing a ScAlMgO4 single crystal substrate according to claim 4, wherein: In the crystal growth step, the temperature gradient just below the liquid surface of the melt is set to 4.4° C. / mm or more.