Ingot cutting method
By measuring the GAP value of the wafer, we judge the reduction in the sharpness of the slurry and adjust the cutting conditions of the ingot, which solves the problem of cutting efficiency reduction caused by the change in the slurry property when the wire saw device cuts the ingot, and improves product qualification rate and production efficiency.
Patent Information
- Application Number
- CN202010312870.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-29
- Filing Date
- 2020-04-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-04-20
AI Technical Summary
When the existing wire saw device cuts the ingot, the cutting efficiency is reduced due to changes in the slurry's physical properties, resulting in deep cutting processing traces and wire marks on the wafer, which affects the product qualification rate and productivity, and is difficult to detect and adjust the cutting conditions in a timely manner.
By measuring the difference (GAP value) between the thickest part and the thinnest part of the inner region of the cut wafer whose central part is smaller than its diameter, we judge the decrease in sharpness of the slurry and adjust the ingot according to the difference value. The cutting conditions, such as reducing the conveying speed, are to suppress the generation of wire marks.
It realizes timely adjustment of cutting conditions when the slurry sharpness decreases, reduces the generation of defective wafers, improves wafer quality and yield, and avoids reduction in productivity and increase in cost.
Smart Images

Figure CN112008902B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ingot cutting method for cutting an ingot made of a brittle material such as silicon, glass, or ceramics using a wire saw device. Background Art
[0002] In recent years, it is expected that wafers will be larger in size, and with this increase in size, a special wire saw device is used to cut the ingot. The wire saw device is a device that cuts the workpiece (for example, a silicon ingot, hereinafter referred to as an ingot) by moving a wire (a high-tension steel wire) at high speed and pressing it against the workpiece while supplying slurry to the wire, so as to simultaneously cut a plurality of wafers from the ingot (for example, refer to Patent Documents 1 and 2).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Publication No. Heisei 9-254143
[0006] Patent Document 2: Japanese Patent Publication No. Heisei 10-81872 Summary of the invention
[0007] 1. Technical issues to be resolved
[0008] When using the above-mentioned wire saw device to cut the ingot, if the cutting efficiency is reduced for some reason, an imbalance will occur between the ingot conveying speed (the speed at which the ingot moves toward the wire) and the speed at which the ingot is actually cut using the wire. As a result, damage will occur on the cut wafer and the processing marks during cutting will deepen.
[0009] When deep cutting marks are produced on the wafer as described above, even if the wafer is ground to a specified thickness in the subsequent CW (chemical etching wafer) process, the processing marks cannot be removed, and the wire marks remain on the wafer, causing defects in the wafer. Defective wafers lose their value, so the pass rate deteriorates, and accordingly, the productivity deteriorates, which is disadvantageous in terms of cost.
[0010] Here, one of the causes of reduced cutting efficiency is the change in the physical properties of the slurry supplied when cutting the ingot, specifically, the change in the particle size of the abrasive grains contained in the slurry, the change in the viscosity, specific gravity, and composition of the slurry, etc.
[0011] In order to suppress the occurrence rate of wire marks caused by the decrease in sharpness (cutting efficiency) caused by the change in the physical properties of the slurry (hereinafter referred to as the decrease in the sharpness of the slurry), it is necessary to change the cutting conditions of the ingot when the sharpness of the slurry decreases. The so-called change in cutting conditions specifically refers to reducing the conveying speed of the ingot and reducing the amount cut per unit time.
[0012] However, even if the physical properties of the slurry are monitored, it is difficult to grasp the reduction in the sharpness of the slurry in detail based on the results, and it is impossible to change the cutting conditions of the ingot based on the monitoring. As a result, after the processing (wafer grinding) in the CW process is completed, the wire mark is found by inspecting the surface of the wafer, and the abnormality is first known. At this time, the cutting conditions of the ingot in the wire saw device can be changed.
[0013] For this reason, during the long period from the ingot cutting in the wire saw process to the detection of abnormality in the surface inspection after the completion of the CW process, the subsequent ingot cutting is performed in a state where the sharpness (cutting efficiency) of the slurry is low, and the wafers cut from the ingot during this period also have the same abnormality of residual wire marks as described above. As a result, a large number of defective wafers are produced.
[0014] Therefore, as a method for detecting a decrease in the sharpness (cutting efficiency) of the slurry, it is conceivable to adopt a method of indirectly detecting the decrease in the sharpness by confirming the degree of bending of the wire rod during the process of cutting the ingot.
[0015] Specifically, if the sharpness is reduced due to the change in the physical properties of the slurry, the distance of pressing the ingot per unit time is longer than the distance of cutting the ingot per unit time, so the wire is bent in a concave shape. By confirming the bending of the wire, the reduction in sharpness can be indirectly detected.
[0016] However, from a safety point of view, it is actually impossible to open the enclosure of the ingot cutting process to measure the bending amount of the wire rod when the slurry is scattered due to the wind pressure generated by the high-speed rotation of the wire guide and the high-speed movement of the wire rod. Therefore, it is considered to temporarily stop the operation of the wire saw device during the ingot cutting to measure the bending amount of the wire rod, but in this case, the wire saw device must be temporarily stopped, which is disadvantageous in terms of productivity. In addition, since the wire saw device is stopped in the middle of the ingot cutting and restarted after the bending amount of the wire rod is measured, the quality of the wafer cut from the ingot may be deteriorated due to this influence.
[0017] In addition, there is also a corresponding method of setting a tool for continuously measuring the wire bending amount while cutting the ingot in a wire saw device, but in this case, the tool must be installed in the wire saw device, which is disadvantageous in terms of installation cost and also causes the problem of large-scale equipment.
[0018] In addition, if the conveying speed of the ingot is set to a low speed from the beginning, even if the sharpness of the slurry deteriorates in the middle of the continuous cutting of the ingot, the wire mark defect accompanying the reduction in sharpness will not occur. However, from the perspective of productivity, it is not a good idea to unnecessarily reduce the conveying speed of the ingot if there is no problem with sharpness.
[0019] Therefore, it is desirable to initially cut the ingot at the highest possible speed, and when the sharpness decreases, immediately detect the decrease and change the cutting conditions, specifically, reduce the ingot conveying speed and reduce the amount cut per unit time.
[0020] The present invention has been made to solve the above-mentioned problems, and an object thereof is to provide a method for cutting an ingot which can immediately detect a decrease in the sharpness of a slurry and thereby change the cutting conditions of the ingot to be cut subsequently immediately after the decrease in the sharpness.
[0021] (II) Technical solution
[0022] In order to achieve the above-mentioned purpose, the present invention provides a method for cutting an ingot, wherein a wire array is formed by wires spirally wound between a plurality of wire guides and moved axially, and the ingot is cut into a wafer shape by supplying slurry to the contact portion between the ingot and the wires while pressing the ingot against the wire array at a specified conveying speed. The method is characterized in that the thickness shape of the wafer cut from the ingot is measured, and the difference between the thickest part and the thinnest part is calculated in a circular area of the cut wafer that includes a central part and has a diameter smaller than the diameter of the cut wafer, and based on the difference, the cutting conditions of the ingot to be cut subsequently are changed.
[0023] According to such an ingot cutting method, a circle including a central portion of a wafer cut from the ingot and having a diameter smaller than the diameter of the cut wafer is newly defined, and the difference between the thickest portion and the thinnest portion in the area within the circle is used as an indicator to change the cutting conditions of the ingot to be cut subsequently, thereby accurately grasping the reduction in the sharpness of the slurry.
[0024] In the past, it was known to use TTV (Total Thickness Variation) as an indicator to represent the deviation of the thickness shape of the wafer. The difference between the thickest part and the thinnest part of the entire wafer surface was used as an indicator to evaluate the flatness of the wafer surface. However, the reduction in sharpness of the slurry cannot be accurately grasped based on this indicator.
[0025] In this regard, as a new indicator for evaluating the reduction in the sharpness of the slurry, the present invention newly defines a circle that includes a central portion of a wafer cut from an ingot and has a diameter smaller than the diameter of the cut wafer as described above, and uses the difference between the thickest portion and the thinnest portion in the area within the circle. This allows the reduction in the sharpness of the slurry to be accurately grasped, and the cutting conditions for the subsequent cutting of the ingot to be changed immediately after the sharpness is reduced.
[0026] In addition, the difference between the thickest part and the thinnest part in the above-mentioned newly defined circle is hereinafter referred to as a "GAP value".
[0027] In addition, it is preferable that the circle be set to a circle having a length corresponding to 1 / 3 or less of the diameter of the cut wafer as a diameter and centered on the center of the cut wafer.
[0028] Thus, the reduction in slurry sharpness can be understood based only on the deviation in the thickness shape of the wafer center portion, which best reflects the reduction in slurry sharpness. Therefore, the reduction in slurry sharpness can be understood more accurately and reflected in the change in the cutting conditions of the ingot to be cut later.
[0029] In addition, it is preferable that the changed cutting condition is set to the conveying speed of the ingot to be cut later.
[0030] This can reduce the amount of cutting per unit time, and can effectively suppress the occurrence rate of wire marks on the diced wafers.
[0031] Furthermore, when the difference is larger than a predetermined value, it is preferable to reduce the conveying speed of the ingot to be cut subsequently.
[0032] Thus, the timing for changing the ingot cutting condition (ingot conveying speed) can be predetermined as a predetermined value. Therefore, the cutting condition can be automatically changed during the operation of the wire saw device, thereby preventing the occurrence of wire marks on the cut wafer without reducing productivity.
[0033] In addition, it is preferable to obtain the difference before the CW process of the cut wafer.
[0034] Thus, the reduction in the sharpness of the slurry can be detected without waiting for the surface inspection after the completion of the CW process. Therefore, when the reduction in sharpness occurs, the cutting conditions of the subsequent ingot can be changed immediately, thereby avoiding the situation where a large number of defective wafers are generated.
[0035] (III) Beneficial effects
[0036] As described above, according to the present invention, a method for cutting an ingot can be realized, which can immediately detect the decrease in the sharpness of the slurry, thereby changing the cutting conditions of the ingot to be cut later immediately after the sharpness decreases. Therefore, the generation of defective wafers can be suppressed and the wafer quality and yield rate can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a schematic diagram showing an example of a wire saw device.
[0038] Figure 2 This is an illustration of TTV.
[0039] Figure 3 This is a diagram illustrating the shape of a wafer.
[0040] Figure 4 This is an illustration of the area within the circle.
[0041] Figure 5 This is a diagram to explain the GAP value.
[0042] Figure 6 This is a flow chart showing an example of the ingot cutting method of the present invention.
[0043] Description of Reference Numerals
[0044] 100-wire saw device; 101-ingot; 102-wire; 103-wire guide; 104, 104'-tension applying mechanism; 105-ingot conveying unit; 106-wire array; 107, 107'-spool; 108-parallel conveying device (Trabasa); 109-fixed torque motor; 110-driving motor; 115-nozzle; 116-slurry tank; 117-heat exchanger. DETAILED DESCRIPTION
[0045] As mentioned above, in the past, as the sharpness (cutting efficiency) decreased due to the change in the physical properties of the slurry, the defect of residual wire marks on the cut wafer occurred. Therefore, the study proposed a method: when the sharpness decreases, the cutting conditions of the ingot to be cut subsequently are changed, thereby suppressing the generation of wire marks thereafter. However, there is the following problem: it is difficult to immediately grasp the decrease in the sharpness of the slurry without increasing the cost, and reflect it in the cutting conditions of the ingot to be cut subsequently.
[0046] Therefore, there has been a demand for developing an ingot cutting method that can immediately detect a decrease in the sharpness of the slurry and change the cutting conditions of the ingot to be cut immediately after the decrease in the sharpness.
[0047] The inventors of the present invention have studied the above problem carefully, and as a result, they have focused on a phenomenon that can be well confirmed when the sharpness of the slurry is reduced. That is, if such a phenomenon is judged, it can be concluded that the sharpness of the slurry is reduced when the phenomenon occurs. However, in order to immediately grasp the reduction in sharpness, it must be a phenomenon that can be observed immediately after the ingot is cut.
[0048] Based on this viewpoint, the inventors further conducted careful research and came to the following conclusion: Regarding the thickness shape (thickness distribution) of the wafer after the ingot is cut, it is effective to use the phenomenon that the deviation (degree of concave and convex) of the thickness shape of the central part of the wafer is greater than that of other parts to grasp the reduction of the sharpness of the slurry. That is, for ordinary wafers cut from the ingot, except for the case where the cutting start part (edge part) is thinner, there is no large concave and convex in other parts (including the central part of the wafer), and it is a roughly flat thickness shape. However, when the sharpness of the slurry is reduced, an uneven area with a mixture of thicker and thinner parts will be generated in the central part of the wafer.
[0049] Furthermore, the range of distance from the center of the wafer in which such thickness deviation occurs was carefully studied, and it was found that the thickness deviation occurs concentratedly in the area outside the edge of the wafer, that is, in the area within a circle whose diameter is smaller than the diameter of the wafer, and especially in the area within a circle whose distance from the center of the wafer is less than 1 / 3 of the radius of the wafer. If the thickness shape of the wafer is measured within this range and the difference between the thickest part and the thinnest part is used as an indicator, the reduction in the sharpness of the slurry can be accurately grasped, thereby completing the present invention.
[0050] That is, the present invention is a method for cutting an ingot, wherein a wire array is formed by wires spirally wound between a plurality of wire guides and moved axially, and the ingot is cut into a wafer shape by supplying slurry to the contact portion between the ingot and the wires while pressing the ingot against the wire array at a prescribed conveying speed. The method is characterized in that the thickness shape of the wafer cut from the ingot is measured, and the difference between the thickest part and the thinnest part is calculated in a circular area of the cut wafer that includes a central part and has a diameter smaller than the diameter of the cut wafer, and based on the difference, the cutting conditions of the ingot to be cut subsequently are changed.
[0051] Hereinafter, embodiments of the present invention will be described in detail based on the drawings, but the present invention is not limited thereto.
[0052] Figure 1 An example of a wire saw device is shown.
[0053] The wire saw device 100 mainly includes: a wire 102, which is used to cut the ingot 101; a wire guide 103, which is wound with the wire 102; a tension applying mechanism 104, 104', which is used to apply tension to the wire 102; an ingot conveying unit 105, which outputs the cut ingot 101; and a nozzle 115, which is used to supply slurry formed by dispersing and mixing abrasive particles in a coolant during cutting.
[0054] The wire 102 is fed from the bobbin 107 on one side, passes through the parallel moving device 108, and then passes through the tension mechanism 104 composed of a magnetic powder clutch (fixed torque motor 109), a tension adjustment roller (deadweight) (not shown), etc., and enters the wire guide 103. The wire 102 is wound around the wire guide 103 for about 300 to 400 turns to form a wire row 106, and then passes through the tension applying mechanism 104' on the other side and is wound on the bobbin 107'.
[0055] The wire guide 103 is a roller having a steel cylinder around which polyurethane resin is pressed and grooves are cut at a constant pitch on its surface, and the wound wire 102 can be driven in a reciprocating direction at a predetermined cycle by a driving motor 110 .
[0056] When the ingot 101 is cut, the ingot 101 is held and pressed by the ingot conveying mechanism 105 and is gradually conveyed at a predetermined conveying speed set in advance.
[0057] A slurry nozzle 115 is provided near the wire 102 wound on the wire guide 103, and slurry can be supplied from a slurry tank 116 to the wire 102 during cutting. In addition, a heat exchanger 117 is connected to the slurry tank 116, and the temperature of the slurry supplied to the wire 102 can be adjusted.
[0058] Using such a wire saw device 101, appropriate tension is applied to the wire 102 by the tension applying mechanism 104, and the wire 102 is moved in a reciprocating direction by the driving motor 110. The ingot 101 is pressed against the wire array 106 while supplying slurry to cut the ingot 101, thereby obtaining a desired cut wafer.
[0059] The obtained cut wafers were cleaned, and after removing the slurry attached to the surface of the wafer and drying, the thickness of the wafer was measured to find the difference between the thickest part and the thinnest part of the circle area including the center.
[0060] Here, TTV is cited as a known indicator for evaluating wafer thickness deviation. TTV is a parameter that quantifies the difference in thickness between the thinnest part and the thickest part of the entire wafer surface. Figure 2As shown in the TTV illustration of FIG, a normal wafer cut from an ingot tends to be thinner at the start of cutting (edge) than at the center of the wafer. That is, TTV is suitable for evaluating the flatness at such an edge, but is not suitable for evaluating the reduction in sharpness of the slurry.
[0061] Therefore, as a phenomenon that can be well confirmed when the sharpness of the slurry is reduced, the phenomenon that the deviation of the thickness shape of the wafer (the degree of unevenness) mainly occurs in the central part of the wafer after cutting is used. Figure 3 As shown in the wafer shape illustration, the thickness shape of a normal wafer after dicing and cutting has a flat thickness shape without much unevenness in other sections except for the thinner portion at the beginning of dicing. In contrast, when the sharpness of the slurry decreases, the thickness shape of the wafer becomes uneven and has a mixed area of thicker and thinner portions not only at the beginning of dicing but also in the center of the wafer.
[0062] Therefore, it is considered that if the thickness deviation in the center of the wafer is understood, it can be determined whether the sharpness of the slurry has been reduced.
[0063] Therefore, as described below, the GAP value, which is different from the TTV, is used as an indicator for evaluating the thickness shape of the wafer after dicing.
[0064] The process of obtaining the GAP value mainly includes: a process of setting an inner region of a circle as a basis for calculating the GAP value; and a process of obtaining the GAP value in the inner region of the circle.
[0065] like Figure 4 As shown in the explanatory diagram of the inner circle area, the inner circle area is set by defining a circle C that includes the center of the cut wafer W and has a diameter smaller than the diameter (2R) of the cut wafer W. The circle C only needs to not include the cutting start portion, and therefore only needs to be smaller than the diameter (2R) of the cut wafer W.
[0066] However, since the deviation of the thickness shape caused by the reduction of the sharpness of the slurry is concentrated in the central part of the wafer W, the circle C is preferably a circle with a length equivalent to 1 / 3 of the diameter (2R) of the cut wafer W and centered on the center O of the cut wafer W. For example, if the diameter of the wafer is 300 mm, it is defined as a circle with a diameter of 100 mm, which is 1 / 3 thereof. In addition, the lower limit of the diameter of the circle C is not particularly limited, and for example, it can be a value greater than 0 mm.
[0067] In addition, if Figure 5 As shown in the figure, the GAP value is defined by Figure 4The difference between the thickest part and the thinnest part in the set circle inner area X. In this way, the deviation of the thickness shape of the cut wafer is obtained as the GAP value without including the cutting start part, so that it is possible to accurately understand whether the sharpness of the slurry has been reduced based on the GAP value.
[0068] In addition, the cut wafer is ground in a CW process such as a grinding and etching process as a subsequent process, and is transported to the subsequent process in a state where the processing marks during cutting and cutting have been removed. However, if deeper processing marks are produced in the cutting process, they cannot be removed in the CW process and will remain on the wafer as wire marks.
[0069] Figure 6 An example of the ingot cutting method of the present invention is shown.
[0070] The following ingot cutting method uses, for example, Figure 1 The wire saw device is performed.
[0071] First, as shown in step S1, the ingot is cut under cutting condition 1 (ingot conveying speed Sx [mm / min]). That is, the ingot is cut by bringing the ingot into contact with the wire rods at the ingot conveying speed Sx while supplying slurry to the contact portion between the ingot and the wire rods.
[0072] Then, as shown in step S2, the thickness shape of the wafer cut from the ingot is measured. Then, as shown in step S3, the GAP value is calculated. As described above, a circle smaller than the diameter of the wafer is set on the surface of the cut wafer, and the difference between the thickest part and the thinnest part in the area within the circle is obtained, so that the GAP value can be calculated.
[0073] Next, as shown in step S4, it is confirmed whether the calculated GAP value is below the specified value. When the GAP value is below the specified value, it is determined that the sharpness of the slurry has not been reduced, and the process returns to step S1. That is, the ingot is cut under the cutting condition 1 for the subsequent batches. On the other hand, when the GAP value is greater than the specified value, it is determined that the sharpness of the slurry has been reduced, and the process proceeds to step S5.
[0074] That is, as shown in step S5, the ingot is cut by switching to the cutting condition 2 (ingot conveying speed Sy [mm / min], Sy < Sx) for the subsequent batch. In addition, as shown in Table 1, when the ingot conveying speed Sx in the cutting condition 1 is set as the reference (100%), the ingot conveying speed Sy in the cutting condition 2 can be 92% of Sx.
[0075]
Table 1
[0076] Changes in cutting conditions
[0077] Ingot conveying speed (when cutting at the center) Cut-off condition 1 100% Cut-off condition 2 92%
[0078] As described above, according to the ingot cutting method of the present invention, as a means of grasping the reduction in sharpness of the slurry (reduction in cutting efficiency) as soon as possible after cutting, a parameter called the GAP value is defined based on the thickness shape of the wafer after cutting. That is, in order to digitize the unevenness confirmed in the central part of the wafer, the GAP value is digitized separately from the TTV representing the thickness deviation of the entire wafer.
[0079] According to the definition of TTV, since the thinnest part of the entire wafer, i.e., the starting part of the wafer cut or the peripheral part of the wire moving direction, is the minimum value of the constraint speed when determining TTV, and the other parts are basically flat, the thickest part in the flat interval is set as the maximum value, and TTV is determined based on the difference between the minimum value and the maximum value. Therefore, when the sharpness of the slurry is reduced as described above, when a deviation (concavity and convexity) in the thickness shape of the wafer is generated, the thickest part is the convex part of the concavity and convexity interval, and the PV (peak-to-valley value) of this part and the thinnest part (the starting part of the cut or the peripheral part) is used to determine TTV.
[0080] However, the thickness of the thinnest part, i.e., the cutting start part or the peripheral part, may also vary due to various reasons. When TTV is large, it is not necessarily possible to determine that the sharpness of the slurry has been reduced. That is, since the thickness deviation (concavity and convexity) of the central part of the wafer is masked by the thickness deviation of the cutting start part or the peripheral part, it is not possible to accurately determine whether the sharpness of the slurry has been reduced by TTV. Therefore, it is difficult to associate TTV with the reduction of the sharpness of the slurry.
[0081] Therefore, as described above, when the sharpness of the slurry is reduced, the GAP value is defined for the purpose of quantifying the unevenness in the wafer surface (excluding the cutting start portion or the outer peripheral portion).
[0082] In addition, the shape of the wafer is usually measured after cutting, but in the ingot cutting method of the present invention, the calculation of the above-mentioned GAP value is newly added to the measurement items, so that the GAP value is monitored in units of batches after cutting. Moreover, based on the GAP value of the cut wafer, the cutting conditions of the batches to be cut later are changed. As the content of the change in the cutting conditions, when the GAP value exceeds the specified value, it is judged that the sharpness of the slurry is reduced, and the ingot conveying speed is reduced.
[0083] In the past, the shape of the wafer was measured after the CW processing was completed. Therefore, when the wire mark was generated, the abnormality of the wafer was discovered and the cutting conditions in the wire saw device were changed. On the other hand, in the ingot cutting method of the present invention, the cutting conditions of the subsequent batches can be changed by measuring immediately after the cutting is completed using the wire saw device. This can suppress the generation of a large number of wire mark defects.
[0084] According to the above ingot cutting method, by immediately understanding the decrease in the sharpness of the slurry, the cutting conditions of the ingot to be cut later can be changed immediately after the decrease in sharpness. Therefore, the generation of defective wafers can be suppressed and the wafer quality can be improved.
[0085] [Example]
[0086] The present invention is described in detail below with reference to the embodiments of the present invention, but the present invention is not limited thereto.
[0087] (Example 1)
[0088] according to Figure 6 The flowchart of the invention cuts the ingot under cutting condition 1 (ingot conveying speed Sx) and calculates the GAP value of the cut wafer. Furthermore, when the GAP value is greater than the specified value, the ingot conveying speed is switched from Sx to Sy, that is, the ingot is cut under cutting condition 2.
[0089] (Comparative Example 1)
[0090] The ingot was cut under the same cutting condition 1 (ingot conveying speed Sx) as in Example 1. In addition, for comparison, the GAP value was calculated for the cut wafers in Comparative Example 1. However, in Comparative Example 1, even when the GAP value was larger than the specified value, the ingot was cut while the ingot conveying speed was always maintained at Sx, that is, the cutting condition 1 was maintained.
[0091] (Verification results)
[0092] Table 2 shows the verification results of Example 1 and Comparative Example 1.
[0093]
Table 2
[0094]
[0095] In Table 2, the table conveying speed is equivalent to the ingot conveying speed. Regarding the numerical value of the table conveying speed, when it is determined that the GAP value is larger than the specified value, it indicates how to set the table conveying speed of the subsequent batch. That is, in Comparative Example 1, even when the GAP value is larger than the specified value, the cutting condition is not changed, and the table conveying speed is kept at 100%. In contrast, in Example 1, when the GAP value is larger than the specified value, the cutting condition is changed, and the table conveying speed is reduced to 92%, and the cutting is performed slower than in Comparative Example 1.
[0096] In this case, as shown in Table 2, it can be seen that in Example 1, compared with Comparative Example 1, for the subsequent batches, the time required to cut one piece becomes longer, the GAP value (average) becomes smaller, and the occurrence rate of wire marks becomes lower.
[0097] Specifically, when the time required to cut a piece in Comparative Example 1 is set to 100%, the GAP value (average) of the wafer after cutting is set to 100%, and the occurrence rate of wafers with wire mark defects after CW processing is set to 100%, in Example 1, although the time required to cut a piece is extended to 108%, the GAP value (average) of the wafer after cutting is reduced to 27%, and the occurrence rate of wafers with wire mark defects after CW processing is reduced to 10%.
[0098] Thus, it was confirmed that in Example 1, the GAP value (center unevenness) of the wafers of the subsequent batch after the cutting conditions were changed was smaller than that of Comparative Example 1, and the wire mark generation rate after CW processing was also suppressed to 1 / 10.
[0099] As described above, according to the present invention, it is possible to realize an ingot cutting method that can change the cutting conditions of the ingot to be cut subsequently immediately after the sharpness is reduced by immediately recognizing the reduction in the sharpness of the slurry.
[0100] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and any scheme having substantially the same structure as the technical idea described in the claims of the present invention and producing the same effects is included in the technical scope of the present invention.
Claims
1. A method for cutting an ingot, comprising forming a wire array by means of wires spirally wound between a plurality of wire guides and moving in an axial direction, supplying a slurry containing abrasive grains to a contact portion between the ingot and the wires, and pressing the ingot against the wire array at a predetermined conveying speed, thereby cutting the ingot into wafers. It is characterized in that measuring the thickness profile of a wafer cut from the ingot, As a circular region including the central portion of the cut wafer and having a diameter smaller than the diameter of the cut wafer, a circular region having a diameter equal to or less than 1 / 3 of the diameter of the cut wafer and centered at the center of the cut wafer is set, and in the circular region, the difference between the thickest portion and the thinnest portion is obtained, Based on the difference, the conveying speed of the ingot to be cut subsequently is changed.
2. The ingot cutting method according to claim 1, characterized in that: When the difference is larger than a predetermined value, the conveying speed of the ingot to be cut subsequently is reduced.
3. The ingot cutting method according to claim 1 or 2, characterized in that: The difference is obtained before the CW process of the cut wafer.
Citation Information
Patent Citations
Precision machining apparatus and precision machining method
CN101237960A
Fabricating method of semiconductor device
CN101599434A
Sapphire substrates and methods of making same
CN101616772A
Equal-line-loss computation method for multi-line cutting machine
CN102626959A
Silicon-block cutting method
CN103448154A