Nickel-containing positive electrode material, preparation method thereof and lithium-ion battery containing the same
Through wet grinding and multi-stage sintering processes, a porous structure nickel-containing positive electrode material is formed, which solves the problems of long sintering time and high energy consumption of the positive electrode material of lithium-ion batteries, and improves the performance and yield of the battery.
Patent Information
- Application Number
- CN202010865478.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-08-25
AI Technical Summary
The sintering process of existing lithium-ion battery positive electrode materials uses oxygen sintering, resulting in problems such as excessive sintering time, low yield and high energy consumption.
Nickel source material, manganese source material and cobalt source material are used to form a porous structure precursor through wet grinding, drying and aerobic sintering. Then, air, air and oxygen mixture and oxygen sintering are used to optimize the sintering process to shorten time and improve production. Rate.
The yield and electrical properties of nickel-containing cathode materials are improved, energy consumption and preparation costs are reduced, structural stability and circulation capacity are enhanced.
Smart Images

Figure CN112079396B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion battery manufacturing, and in particular to a nickel-containing positive electrode material, a preparation method thereof and a lithium ion battery comprising the same. Background Art
[0002] As the nickel content of high-nickel cathode materials increases, they also bring more problems, such as low safety performance, poor cycle performance, and reduced rate performance. Therefore, the market is still continuously improving the performance of 8-series high-nickel ternary materials.
[0003] In order to solve the above problems, the existing method mainly prepares the ternary precursor by coprecipitation method first, and then mixes it with lithium source to synthesize the material by high temperature solid phase method. The calcination process of ternary material is an oxidation process, which is controlled by the cation diffusion rate. A large amount of oxygen gathers on the surface, which will increase the cation vacancies, which is conducive to the acceleration of cation diffusion and the promotion of calcination, and proceeds in the positive reaction direction. Therefore, providing the necessary oxygen partial pressure will increase the diffusion and solubility of the gas in the pores of the material during the calcination of the ternary material, so that the substances can fully react and increase the reaction rate. At present, the general practice is to use oxygen sintering during the material sintering process, and the sintering time is too long, which has the disadvantages of low yield and high energy consumption.
[0004] In view of the above problems, it is necessary to provide a method for preparing a nickel-containing positive electrode material with high sintering efficiency, low energy consumption and high yield of nickel-containing positive electrode material. Summary of the invention
[0005] The main purpose of the present invention is to provide a nickel-containing positive electrode material, a preparation method thereof and a lithium-ion battery containing the same, so as to solve the problems that the sintering process of the existing positive electrode material preparation method uses oxygen sintering, the sintering time is too long, the yield is low, the energy consumption is high, etc.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a nickel-containing positive electrode material on the one hand, and the method for preparing a nickel-containing positive electrode material comprises: a nickel source material, a manganese source material, a cobalt source material and a first dopant are subjected to a wet grinding, drying and aerobic sintering process in sequence to obtain a precursor with a porous structure; the precursor, a lithium source material and a second dopant are subjected to an air sintering process, an air and oxygen mixed gas sintering process and an oxygen sintering process in sequence, and after the reaction is completed, the mixture is cooled to obtain a nickel-containing positive electrode material.
[0007] Furthermore, the aerobic sintering process is a programmed temperature rising process. Preferably, the temperature rising process of aerobic sintering includes: heating to 120-260°C at 2-10°C / min, keeping warm for 100-130min, then heating to 400-500°C at 2-10°C / min, keeping warm for 180-220min, and cooling naturally.
[0008] Furthermore, in the mixed gas of air and oxygen, the content of oxygen is 21 to 99.99%.
[0009] Furthermore, the heating rates of the air sintering process, the air and oxygen mixed gas sintering process and the oxygen sintering process are 2 to 10°C / min; preferably, the air sintering process includes: subjecting the precursor having a porous structure to a first constant temperature sintering process at a first sintering temperature to obtain a first constant temperature sintering product, wherein the sintering temperature of the first constant temperature sintering process is 120°C to 260°C, and the sintering time is 60 to 120 min; subjecting the first constant temperature sintering product to a second constant temperature sintering process at a second sintering temperature to obtain a second constant temperature sintering product, wherein the sintering temperature of the second constant temperature sintering process is 300 to 360°C, and the sintering time is 120 to 200 min.
[0010] Furthermore, the sintering process of the mixed gas of air and oxygen includes: performing a third constant temperature sintering process on the second constant temperature sintering product at a third constant temperature sintering temperature to obtain a third constant temperature sintering product, wherein the temperature of the third constant temperature sintering process is 480-520°C, and the sintering time is 200-300min; performing a fourth constant temperature sintering process on the third constant temperature sintering product at a fourth constant temperature sintering temperature to obtain a fourth constant temperature sintering product, wherein the sintering temperature of the fourth constant temperature sintering process is 600-650°C, and the sintering time is 60-120min.
[0011] Furthermore, the oxygen sintering process includes: performing a fifth constant temperature sintering process on the fourth constant temperature sintering product at a fifth constant temperature sintering temperature to obtain a fifth constant temperature sintering product, wherein the temperature of the fifth constant temperature sintering process is 650-690°C, and the sintering time is 100-200min; performing a sixth constant temperature sintering process on the fifth constant temperature sintering product at a sixth constant temperature sintering temperature to obtain a sixth constant temperature sintering product, wherein the sintering temperature of the sixth constant temperature sintering process is 695-810°C, and the sintering time is 600-690min; performing a seventh constant temperature sintering process on the sixth constant temperature sintering product at a seventh constant temperature sintering temperature to obtain a nickel-containing positive electrode material, wherein the sintering temperature of the seventh constant temperature sintering process is reduced from 800°C to 600°C, and the sintering time is 100-500min.
[0012] Furthermore, the preparation method also includes: crushing and screening the product system of the seventh constant temperature sintering process to obtain a nickel-containing positive electrode material; preferably, the screening mesh size used in the screening process is 300 mesh to 400 mesh.
[0013] Furthermore, the weight ratio of the lithium source material to the precursor is (1.00-1.15):1, the weight of the metal element in the first dopant is 0.05-5% of the weight of the nickel element in the precursor, and the weight of the metal element in the second dopant is 0.05-1% of the weight of the nickel element in the precursor; preferably, the nickel source material is selected from one or more of the group consisting of nickel hydroxide, nickel oxide and nickel carbonate; preferably, the manganese source material is selected from one or more of the group consisting of manganese carbonate, manganese hydroxide and manganese oxide; preferably, the cobalt source material is selected from one or more of the group consisting of cobalt hydroxide, cobalt oxide and cobalt carbonate; preferably, the first dopant and the second dopant are independently selected from one or more of the group consisting of aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, magnesium carbonate, titanium dioxide and titanium hydroxide.
[0014] Furthermore, the precursor of the porous structure is spherical, and the particle size is 1-28 μm; preferably, the precursor of the porous structure is formed by agglomeration of primary particles, and the particle size of the primary particles is 20-300 nm.
[0015] Furthermore, the drying process is a spray drying process. Preferably, the spray drying device used in the spray drying process has an inlet temperature of 275-290°C, an outlet temperature of 105-119°C, a compressed air pressure of 0.3-0.5Mpa, and an air flow rate of 3.5-7.5m 3 / h.
[0016] Another aspect of the present application further provides a nickel-containing positive electrode material, which is prepared by the above-mentioned preparation method.
[0017] Another aspect of the present application provides a lithium-ion battery, including a positive electrode material, wherein the positive electrode material includes the nickel-containing positive electrode material provided in the present application.
[0018] By applying the technical solution of the present invention, the nickel source material, the manganese source material, the cobalt source material and the first dopant are wet-ground to the desired particle size, and spherical particles are formed through a drying process. Then, the spherical particles are melted and agglomerated through an aerobic sintering process to obtain a ternary precursor in which multiple oxides coexist, and the ternary precursor has a porous structure. Finally, the mixture of the ternary precursor, the lithium source material and the second dopant is sequentially subjected to an air sintering process, an air-oxygen mixed gas sintering process and an oxygen sintering process, which can make the reactants and the atmosphere contact more fully, optimize the sintering process, thereby shortening the sintering time, reducing the amount of oxygen used, and improving the yield of the nickel-containing positive electrode material. At the same time, combining the first dopant and the second dopant with the above process is also beneficial to improving the electrical properties such as the structural stability, energy density and cycle capacity of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0020] Figure 1 The SEM image of the precursor prepared in Example 1 of the present invention obtained at a magnification of 50,000 times is shown;
[0021] Figure 2 The SEM image of the precursor prepared in Example 1 of the present invention is obtained at a magnification of 10000 times;
[0022] Figure 3 The graph shows the cycle data of the nickel-containing positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0024] As described in the background technology, in the existing preparation method of positive electrode materials, oxygen sintering is used in the sintering process, and the sintering time is too long, and there are problems such as low yield and high energy consumption. In order to solve the above technical problems, the present application provides a method for preparing a nickel-containing positive electrode material, and the preparation method of the nickel-containing positive electrode material comprises: a nickel source material, a manganese source material, a cobalt source material and a first dopant are sequentially subjected to wet grinding, drying and aerobic sintering processes to obtain a precursor with a porous structure; the precursor, the lithium source material and the second dopant are sequentially subjected to an air sintering process, a mixed gas sintering process of air and oxygen and an oxygen sintering process, and after the reaction is completed, cooling is performed to obtain a nickel-containing positive electrode material.
[0025] The nickel source material, manganese source material, cobalt source material and the first dopant are wet-grinded to the desired particle size, and spherical particles are formed through a drying process. Then, the spherical particles are melted and agglomerated through an aerobic sintering process to obtain a ternary precursor in which multiple oxides coexist, and the ternary precursor has a porous structure. Finally, the mixture of the ternary precursor, the lithium source material and the second dopant is subjected to an air sintering process, an air-oxygen mixed gas sintering process and an oxygen sintering process in sequence, which can make the reactants and the atmosphere contact more fully, optimize the sintering process, thereby shortening the sintering time, reducing the amount of oxygen used, and improving the yield of the nickel-containing positive electrode material. At the same time, combining the first dopant and the second dopant with the above process is also beneficial to improving the electrical properties such as the structural stability, energy density and cycle capacity of the positive electrode material.
[0026] In a preferred embodiment, the aerobic sintering process is a programmed temperature rising process, preferably, the temperature is raised to 120-260°C at 2-10°C / min, kept at this temperature for 100-130min, then raised to 400-500°C at 2-10°C / min, kept at this temperature for 180-220min, and cooled naturally. The above-mentioned aerobic sintering process is beneficial to further improve the structural stability and specific surface area of the precursor, thereby further reducing the amount of oxygen used, shortening the sintering time, and improving the electrical properties and yield of the nickel-containing positive electrode material.
[0027] Preferably, the oxygen content in the mixed gas of air and oxygen is 21-99.99%.
[0028] In a preferred embodiment, the heating rate of the air sintering process, the mixed gas sintering process of air and oxygen, and the oxygen sintering process is 2 to 10°C / min. The heating rate of the air sintering process, the mixed gas sintering process of air and oxygen, and the oxygen sintering process includes but is not limited to the above range, and limiting it to the above range is conducive to improving the full reaction degree of each sintering stage, thereby facilitating further improving the yield of the nickel-containing positive electrode material.
[0029] In the above preparation method, the sintering temperature of the air sintering process, the temperature of the mixed gas of air and oxygen sintering process, and the temperature of the oxygen sintering process are increased in sequence. Preferably, the sintering temperature of the air sintering process, the temperature of the mixed gas of air and oxygen sintering process, and the temperature of the oxygen sintering process are in the range of 120 to 600°C.
[0030] In a preferred embodiment, the air sintering process includes: subjecting a precursor having a porous structure to a first constant temperature sintering process at a first sintering temperature to obtain a first constant temperature sintering product, wherein the sintering temperature of the first constant temperature sintering process is 120 to 260°C, and the sintering time is 60 to 120 minutes; subjecting the first constant temperature sintering product to a second constant temperature sintering process at a second sintering temperature to obtain a second constant temperature sintering product, wherein the sintering temperature of the second constant temperature sintering process is 300 to 360°C, and the sintering time is 120 to 360 minutes.
[0031] In a preferred embodiment, the sintering process of the mixed gas of air and oxygen includes: performing a third constant temperature sintering process on the second constant temperature sintering product at a third constant temperature sintering temperature to obtain a third constant temperature sintering product, wherein the temperature of the third constant temperature sintering process is 480-520°C, and the sintering time is 200-300 minutes; performing a fourth constant temperature sintering process on the third constant temperature sintering product at a fourth constant temperature sintering temperature to obtain a fourth constant temperature sintering product, wherein the sintering temperature of the fourth constant temperature sintering process is 600-650°C, and the sintering time is 60-120 minutes.
[0032] In a preferred embodiment, the oxygen sintering process includes: performing a fifth constant temperature sintering process on the fourth constant temperature sintering product at a fifth sintering temperature to obtain a fifth constant temperature sintering product, wherein the temperature of the fifth constant temperature sintering process is 650-690°C, and the sintering time is 100-200 min; performing a sixth constant temperature sintering process on the fifth constant temperature sintering product at a sixth constant temperature sintering temperature to obtain a sixth constant temperature sintering product, wherein the sintering temperature of the sixth constant temperature sintering process is 695-810°C, and the sintering time is 600-690 min; performing a seventh constant temperature sintering process on the sixth constant temperature sintering product at a seventh constant temperature sintering temperature to obtain a nickel-containing positive electrode material, wherein the sintering temperature of the seventh constant temperature sintering process is reduced from 800°C to 600°C, and the sintering time is 100-500 min.
[0033] Limiting the specific processes of the air sintering process, the air and oxygen mixed gas sintering process, and the oxygen sintering process within the above range is beneficial to further improve the degree of contact between the reaction raw materials and the atmosphere, shorten the sintering time, and further improve the yield of the nickel-containing positive electrode material.
[0034] In a preferred embodiment, the preparation method further includes: crushing and screening the product system of the seventh constant temperature sintering process to obtain a nickel-containing positive electrode material. After crushing and screening, the particle size of the nickel-containing positive electrode material is smaller and more uniform. Compared with the positive electrode material obtained without crushing and screening, the nickel-containing positive electrode material obtained after the above treatment can fully contact and react with the electrolyte, and there are fewer side reactions, so that it has a better cycle capacity. More preferably, the screening mesh number used in the screening process is 300 mesh to 400 mesh.
[0035] In a preferred embodiment, the weight ratio of the lithium source material to the precursor is (1.00-1.15):1, the weight of the metal element in the first dopant is 0.05-5% of the weight of the nickel element in the precursor, and the weight of the metal element in the second dopant is 0.05-1% of the weight of the nickel element in the precursor. The weight ratio of the lithium source material to the precursor and the content of the metal element in the first dopant and the second dopant include but are not limited to the above ranges, and limiting them within the above ranges is conducive to further improving the electrochemical capacity and cycle performance of the positive electrode material.
[0036] In the above preparation method, the nickel source material, manganese source material, lithium source material, first dopant and second dopant can be selected from the commonly used types in the art. Preferably, the nickel source material includes but is not limited to one or more of the group consisting of nickel hydroxide, nickel oxide and nickel carbonate; preferably, the manganese source material includes but is not limited to one or more of the group consisting of manganese carbonate, manganese hydroxide and manganese oxide; preferably, the cobalt source material includes but is not limited to one or more of the group consisting of cobalt hydroxide, cobalt oxide and cobalt carbonate; preferably, the first dopant and the second dopant are independently selected from one or more of the group consisting of aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, magnesium carbonate, titanium dioxide and titanium hydroxide.
[0037] In a preferred embodiment, the precursor of the porous structure is spherical and has a particle size of 1 to 28 nm. The particle size of the precursor with a porous structure includes but is not limited to the above range, and limiting it within the above range can further increase its contact area with the lithium source, the second doping agent and the sintering atmosphere, thereby helping to further reduce the amount of oxygen used and improve the yield of the nickel-containing positive electrode material. More preferably, the precursor with a porous structure is formed by agglomeration of primary particles, and the particle size of the primary particles is 20 to 300 nm. Limiting the particle size of the first particles within the above range is beneficial to further improve the structural stability of the nickel-containing positive electrode material.
[0038] In the above preparation method, the raw material that forms the precursor during the drying process forms spherical particles. In a preferred embodiment, the drying process is a spray drying process. The use of a spray drying method for drying is beneficial to increasing the proportion of spherical particles in the material obtained after drying, thereby further reducing the amount of oxygen used. More preferably, the inlet temperature of the spray drying device used in the spray drying process is 275-290°C, the outlet temperature is 105-119°C, the compressed air pressure is 0.3-0.5Mpa, and the air intake flow rate is 3.5-7.5m 3 / h. Limiting the process parameters of the spray drying process within the above range is not only conducive to further improving the efficiency of spray drying, but also conducive to further increasing the proportion of spherical particles of the material obtained after drying, thereby further reducing the amount of oxygen used and the electrical properties of the nickel-containing positive electrode material.
[0039] Preferably, the wet grinding process can adopt the process commonly used in the art, such as grinding under the action of solvents such as ethanol and water.
[0040] Another aspect of the present application further provides a nickel-containing positive electrode material, which is prepared by the above-mentioned preparation method.
[0041] The nickel source material, manganese source material, cobalt source material and the first dopant are wet-ground to the desired particle size, and spherical particles are formed through a drying process. Then, the spherical particles are melted and agglomerated through an aerobic sintering process to obtain a ternary precursor in which multiple oxides coexist, and the ternary precursor has a porous structure. Finally, the mixture of the ternary precursor, the lithium source and the second dopant is sequentially subjected to an air sintering process, an air-oxygen mixed gas sintering process and an oxygen sintering process, which can make the reactants and the atmosphere contact more fully, optimize the sintering process, thereby shortening the sintering time, reducing the amount of oxygen used, and improving the yield of the nickel-containing positive electrode material. At the same time, combining the first dopant and the second dopant with the above process is also beneficial to improving the electrical properties such as the structural stability, energy density and cycle capacity of the positive electrode material.
[0042] Another aspect of the present application further provides a lithium-ion battery, comprising a positive electrode material, wherein the positive electrode material comprises the nickel-containing positive electrode material provided in the present application.
[0043] Since the above nickel-containing positive electrode materials have the advantages of low energy consumption, low preparation cost, stable structure and excellent electrical properties, using them to prepare lithium-ion batteries can greatly reduce their costs, while also improving their performance stability, electrical properties and service life.
[0044] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0045] Example 1
[0046] The implementation steps of the present invention are as follows:
[0047] The raw materials are nickel hydroxide, cobalt hydroxide, manganese carbonate and a doping agent, and deionized water is added to prepare a slurry with a solid content of 15%. The doping agent is aluminum hydroxide, and the content of aluminum element is 0.5% of the content of nickel element.
[0048] The slurry was dispersed for 2 hours using a high-speed disperser at 1500 rpm, and then ground for 2 hours using a ball mill. The ball-milled material was spray dried, and the inlet temperature of the spray device was set to 275°C, the outlet temperature to 105°C, the compressed air pressure to 0.3Mpa, and the air flow rate to 3.5m 3 / h, to prepare a ternary mixture.
[0049] The above ternary mixture was placed in a muffle furnace for heating and sintering. The heating rate was set to 10°C / min and the temperature was raised to 120°C. The temperature was kept at this temperature for 100 minutes. Then the temperature was raised to 400°C at 10°C / min and kept at this temperature for 180 minutes. The ternary precursor was naturally cooled to obtain the ternary precursor. The ternary precursor obtained by this method is a primary particle agglomerate with a loose porous structure. The primary particles are about 200nm, and the primary particles are filled with voids. The D(50) is 8.6μm and the specific surface area is 3.85m 2 / g.
[0050] The above-mentioned ternary precursor, lithium source and doping agent (wherein the doping agent is aluminum hydroxide, and the amount of aluminum element is 0.05% of the nickel element content) are mixed in a certain proportion, and the lithium ratio (lithium source / precursor) is 1.05:1. Use a ball mill or a high-speed mixer for mixing, wherein the speed of the ball mill mixing is 300 rpm, the ball milling medium used is made of zirconium oxide, and the weight of the zirconium balls used is 1.5 times the amount of the material. The powder after mixing is loaded into a special sagger for ternary materials, the loading amount is 400g, the loading method is flat, and the sagger used is a chrysocolla mullite ceramic composite material, which is a sagger with legs. The sagger filled with the material is placed in an atmosphere muffle furnace for sintering to obtain a nickel-containing positive electrode material, wherein the heating rate during sintering is 2°C / min. The constant temperature time and sintering atmosphere of the multi-atmosphere sintering process are shown in Table 1.
[0051] The SEM image of the precursor prepared in Example 1 obtained at a magnification of 50,000 times is shown in Figure 1 , SEM images obtained at a magnification of 50,000 times are shown in Figure 2 , the electrical cycle performance data of nickel-containing positive electrode materials can be found in Figure 3 .
[0052] Table 1
[0053] temperature 120℃ 300℃ 480℃ 600℃ 680℃ 700℃ 650℃ Constant temperature time 60min 120min 200min 60min 60min 480min 110min Air flow 2L / min 4L / min 4.5L / min 1L / min 2L / min 2L / min 2L / min atmosphere Air Air Mixed gas Mixed gas oxygen oxygen oxygen
[0054] Among them, the oxygen content is 30% at 480°C and 60% at 600°C.
[0055] After sintering is completed, the temperature naturally drops to 100°C, and the material is taken out. The taken out material is crushed by a machine crusher. After crushing, it is sieved by a vibration sieving instrument with a mesh size of 300 to obtain a nickel-containing positive electrode material.
[0056] Performance Test:
[0057] The nickel-containing positive electrode material prepared in this embodiment is used as the positive electrode active material, acetylene black is used as the conductive agent, polyvinylidene fluoride is used as the binder, the weight ratio of the three is 90:5:5, the lithium sheet is used as the negative electrode, the separator is celgard 2300, and the batteries are assembled into button cells.
[0058] 1 mol / L LiPF6 conductive salt and DMC:DEC:EC weight ratio of 1:1:1 solvent were used as the electrolyte. Under the conditions of 0.1C / 0.1C, 3-4.3V charge and discharge, the measured discharge capacity was 205mAh / g, and the first efficiency was 87.87%. The number of cycles under the conditions of 3-4.3V, 0.1C / 0.1C was 50, and the capacity retention rate was 97.3%.
[0059] Example 2
[0060] The implementation steps of the present invention are as follows:
[0061] The raw materials are nickel hydroxide, cobalt hydroxide, manganese carbonate, and a doping agent titanium dioxide. Ethanol is added to prepare a slurry with a solid content of 25%, wherein the doping agent is titanium dioxide, and the molar ratio of nickel hydroxide:cobalt hydroxide:manganese carbonate:titanium dioxide is 160:17:20:1.
[0062] The slurry was dispersed for 2.5 hours using a high-speed disperser at 1500 rpm, and then ground for 3 hours using a ball mill. The ball-milled material was spray dried, and the inlet temperature of the spray device was set to 285°C, the outlet temperature to 110°C, the compressed air pressure to 0.5 MPa, and the air flow rate to 4.5 m 3 / h. A ternary mixture is prepared.
[0063] The above ternary mixture and lithium source were placed in a muffle furnace for heating and sintering. The heating rate was set to 10°C / min to 120°C, and the temperature was kept for 100 minutes. Then the temperature was raised to 400°C at 10°C / min, and the temperature was kept for 180 minutes. The ternary precursor was naturally cooled to obtain the ternary precursor. The ternary precursor obtained by this method is a primary particle agglomerate with a loose porous structure, a spherical D(50) of 9.2μm, a primary particle of about 250nm, a void structure between the primary particles, and a specific surface area of 3.62m 2 / g.
[0064] The precursor, lithium source and doping agent (wherein the doping agent is magnesium hydroxide, and the content of magnesium element is 0.07% of the content of nickel element) are mixed in a certain proportion, and the lithium ratio (lithium source / precursor) is 1.07:1. Use a ball mill or a high-speed mixer for mixing, wherein the speed of the high-speed mixer is 1000 rpm, and the mixing time is 2min. The powder after mixing is loaded into a special sagger for ternary materials, the loading amount is 500g, the loading method is flat, and the sagger used is a chrysocolla mullite ceramic composite material, which is a sagger with legs. The sagger containing the material is placed in an atmosphere muffle furnace for sintering. The heating rate during sintering is 2°C / min. The constant temperature time and sintering atmosphere of the multi-atmosphere sintering process are shown in Table 2.
[0065] Table 2
[0066] temperature 120℃ 300℃ 480℃ 600℃ 670℃ 720℃ 670℃ Constant temperature time 60min 120min 200min 60min 60min 480min 110min Air flow 2L / min 4L / min 4.5L / min 1L / min 2L / min 2L / min 2L / min atmosphere Air Air Mixed gas Mixed gas oxygen oxygen oxygen
[0067] Among them, the oxygen content is 30% at 480°C and 60% at 600°C.
[0068] After sintering is completed, the temperature naturally drops to 100°C, and the material is taken out. The taken out material is crushed by a machine crusher. After crushing, it is screened by a vibrating screener with a mesh size of 300.
[0069] Performance Test:
[0070] The nickel-containing positive electrode material prepared in this embodiment is used as the positive electrode active material, acetylene black is used as the conductive agent, polyvinylidene fluoride is used as the binder, the weight ratio of the three is 90:5:5, the lithium sheet is used as the negative electrode, the separator is celgard 2300, and the batteries are assembled into button cells.
[0071] 1 mol / L LiPF6 conductive salt and DMC:DEC:EC (wt%) with a weight ratio of 1:1:1 were used as the electrolyte. Under the conditions of 0.1C / 0.1C, 3-4.3V charge and discharge, the measured discharge capacity was 202mAh / g, and the first efficiency was 87.52%. The number of cycles under the conditions of 3-4.3V, 0.1C / 0.1C was 50, and the capacity retention rate was 97.2%.
[0072] Example 3
[0073] The difference from Example 1 is that the inlet temperature of the spray drying process is 275°C, the outlet temperature is 119°C, the compressed air pressure is 0.3 MPa, and the air flow rate is 3.5 m 3 / h.
[0074] The particle size of the primary particles in the spherical precursor is 8.7 nm, and the specific surface area of the spherical precursor is 3.5 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 97.3%.
[0075] Example 4
[0076] The difference from Example 1 is that the inlet temperature of the spray drying process is 290°C, the outlet temperature is 105°C, the compressed air pressure is 0.5 MPa, and the air flow rate is 7.5 m 3 / h.
[0077] The particle size of the primary particles in the spherical precursor is 10.2 nm, and the specific surface area of the spherical precursor is 2.9 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 94.2%.
[0078] Example 5
[0079] The difference from Example 1 is that the inlet temperature of the spray drying process is 300°C, the outlet temperature is 125°C, the compressed air pressure is 0.1 MPa, and the air flow rate is 3m 3 / h.
[0080] The particle size of the primary particles in the spherical precursor is 10.5 nm, and the specific surface area of the spherical precursor is 2.7 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 84.2%.
[0081] Example 6
[0082] The difference from Example 1 is that the heating process of oxygen sintering includes: heating to 170°C at a heating rate of 3°C / min, keeping warm for 60 minutes, then heating to 720°C at a heating rate of 5°C / min, keeping warm for 600 minutes, and cooling naturally.
[0083] The particle size of the primary particles in the spherical precursor is 10.2 nm, and the specific surface area of the spherical precursor is 3.2 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 95.2%.
[0084] Example 7
[0085] The difference from Example 1 is that the heating process of oxygen sintering includes: heating to 260°C at a heating rate of 5°C / min, keeping warm for 120min, then heating to 500°C at a heating rate of 10°C / min, keeping warm for 200min, and cooling naturally.
[0086] The particle size of the primary particles in the spherical precursor is 200 nm, and the specific surface area of the spherical precursor is 3.86 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 97.2%.
[0087] Example 8
[0088] The constant temperature time and sintering atmosphere of the multi-atmosphere sintering process are shown in Table 3.
[0089] Table 3
[0090]
[0091] The particle size of the primary particles in the spherical precursor is 240 nm, and the specific surface area of the spherical precursor is 3.75 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 96.7%.
[0092] Example 9
[0093] The constant temperature time and sintering atmosphere of the multi-atmosphere sintering process are shown in Table 4.
[0094] Table 4
[0095]
[0096] The particle size of the primary particles in the spherical precursor is 250 nm, and the specific surface area of the spherical precursor is 3.51 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 96.9%.
[0097] Example 10
[0098] The constant temperature time and sintering atmosphere of the multi-atmosphere sintering process are shown in Table 5.
[0099] Table 5
[0100]
[0101] The particle size of the primary particles in the spherical precursor is 280 nm, and the specific surface area of the spherical precursor is 3.41 m 2 / g, the cycle number of the nickel-containing positive electrode material is 50, and the capacity retention rate is 90.8%.
[0102] From the above description, it can be seen that the above-mentioned embodiment of the present invention achieves the following technical effects: the nickel source material, the manganese source material, the cobalt source material and the first dopant are wet-ground to the desired particle size, and spherical particles are formed through a drying process, and then the spherical particles are melted and agglomerated through an aerobic sintering process to obtain a ternary precursor in which multiple oxides coexist, and the ternary precursor has a porous structure. Finally, the mixture of the above-mentioned ternary precursor, the lithium source material and the second dopant is subjected to an air sintering process, an air and oxygen mixed gas sintering process and an oxygen sintering process in sequence, which can make the reactants and the atmosphere contact more fully, optimize the sintering process, thereby shortening the sintering time, reducing the amount of oxygen used, and improving the yield of the nickel-containing positive electrode material. At the same time, combining the first dopant and the second dopant with the above-mentioned process is also beneficial to improving the electrical properties such as the structural stability, energy density and cycle capacity of the positive electrode material.
[0103] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a nickel-containing positive electrode material, characterized in that: The preparation method of the nickel-containing positive electrode material comprises: The nickel source material, the manganese source material, the cobalt source material and the first dopant are sequentially subjected to wet grinding, drying and oxygen sintering processes to obtain a precursor with a porous structure; The precursor, the lithium source material and the second dopant are subjected to an air sintering process, an air-oxygen mixed gas sintering process and an oxygen sintering process in sequence, and after the reaction is completed, the mixture is cooled to obtain the nickel-containing positive electrode material; The drying process is a spray drying process; the spray drying device used in the spray drying process has an inlet temperature of 275-290°C, an outlet temperature of 105-119°C, a compressed air pressure of 0.3-0.5 Mpa, and an air flow rate of 3.5-7.5 m 3 / h; The heating process of the oxygen sintering includes: heating to 120-260° C. at 2-10° C. / min, keeping the temperature for 100-130 minutes, then heating to 400-500° C. at 2-10° C. / min, keeping the temperature for 180-220 minutes, and cooling naturally.
2. The method for preparing a nickel-containing positive electrode material according to claim 1, characterized in that: The content of oxygen in the mixed gas of air and oxygen is 21-99.99%.
3. The method for preparing a nickel-containing positive electrode material according to claim 2, characterized in that: The heating rates of the air sintering process, the mixed gas sintering process of air and oxygen, and the oxygen sintering process are 2 to 10°C / min; The air sintering process comprises: The precursor having a porous structure is subjected to a first constant temperature sintering process at a first sintering temperature to obtain a first constant temperature sintering product, wherein the sintering temperature of the first constant temperature sintering process is 120° C. to 260° C., and the sintering time is 60 to 120 min; The first constant temperature sintered product is subjected to a second constant temperature sintering process at a second sintering temperature to obtain a second constant temperature sintered product, wherein the sintering temperature of the second constant temperature sintering process is 300-360° C. and the sintering time is 120-200 min.
4. The method for preparing a nickel-containing positive electrode material according to claim 3, characterized in that: The mixed gas sintering process of air and oxygen comprises: The second constant temperature sintered product is subjected to a third constant temperature sintering process at a third sintering temperature to obtain a third constant temperature sintered product, wherein the temperature of the third constant temperature sintering process is 480-520° C., and the sintering time is 200-300 min; The third constant temperature sintered product is subjected to a fourth constant temperature sintering process at a fourth constant temperature sintering temperature to obtain a fourth constant temperature sintered product, wherein the sintering temperature of the fourth constant temperature sintering process is 600-650° C., and the sintering time is 60-120 min.
5. The method for preparing a nickel-containing positive electrode material according to claim 4, characterized in that: The oxygen sintering process comprises: The fourth constant temperature sintered product is subjected to a fifth constant temperature sintering process at a fifth sintering temperature to obtain a fifth constant temperature sintered product, wherein the temperature of the fifth constant temperature sintering process is 650-690° C., and the sintering time is 100-200 min; The fifth constant temperature sintered product is subjected to a sixth constant temperature sintering process at a sixth constant temperature sintering temperature to obtain a sixth constant temperature sintered product, wherein the sintering temperature of the sixth constant temperature sintering process is 695-810° C., and the sintering time is 600-690 min; The sixth constant temperature sintering product is subjected to a seventh constant temperature sintering process at a seventh constant temperature sintering temperature to obtain the nickel-containing positive electrode material, wherein the sintering temperature of the seventh constant temperature sintering process is reduced from 800° C. to 600° C., and the sintering time is 100 to 500 minutes.
6. The method for preparing a nickel-containing positive electrode material according to claim 5, characterized in that: The preparation method further includes: crushing and screening the product system of the seventh constant temperature sintering process to obtain the nickel-containing positive electrode material. 7 . The method for preparing a nickel-containing positive electrode material according to claim 6 , wherein the sieving mesh size used in the sieving process is 300-400 mesh.
8. The method for preparing a nickel-containing positive electrode material according to any one of claims 1 to 7, characterized in that: The weight ratio of the lithium source material to the precursor is (1.00-1.15): 1, the weight of the metal element in the first dopant is 0.05-5% of the weight of the nickel element in the precursor, and the weight of the metal element in the second dopant is 0.05-1% of the weight of the nickel element in the precursor.
9. The method for preparing a nickel-containing positive electrode material according to claim 8, characterized in that: The nickel source material is selected from one or more of the group consisting of nickel hydroxide, nickel oxide and nickel carbonate; and / or the manganese source material is selected from one or more of the group consisting of manganese carbonate, manganese hydroxide and manganese oxide; and / or The cobalt source material is selected from one or more of the group consisting of cobalt hydroxide, cobalt oxide and cobalt carbonate; and / or The first dopant and the second dopant are independently selected from one or more of the group consisting of aluminum hydroxide, aluminum oxide, magnesium hydroxide, magnesium oxide, magnesium carbonate, titanium dioxide and titanium hydroxide.
10. The method for preparing a nickel-containing positive electrode material according to claim 1, characterized in that: The precursor of the porous structure is spherical and has a particle size of 1 to 28 μm.
11. The method for preparing a nickel-containing positive electrode material according to claim 10, characterized in that: The precursor of the porous structure is formed by agglomeration of primary particles, and the particle size of the primary particles is 20-300 nm.
12. A nickel-containing positive electrode material, characterized in that: The nickel-containing positive electrode material is prepared by the preparation method described in any one of claims 1 to 11.