Composition for forming composite solid electrolyte, composite solid electrolyte membrane and battery containing the same
By using a combination of polyurethane with specific molecular weight and hardness and lithium salt or sodium salt to prepare a composite solid electrolyte membrane, the trade-off problem between ionic conductivity, thermal stability and mechanical strength of the solid electrolyte is solved, and high conductivity is achieved , good mechanical properties and low-cost battery electrolytes.
Patent Information
- Application Number
- CN202011173545.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Existing solid electrolytes cannot simultaneously satisfy high ionic conductivity, thermal stability and good mechanical strength.
A combination of polyurethane and conductive metal salt (such as lithium salt or sodium salt) is used. The weight average molecular weight of polyurethane is 100,000 to 110,000, the hardness is 90 to 100 Shore A, and the tensile strength is 35 to 40MPa. The lithium salt or sodium salt is The solubility is limited to a specific range, and the composite solid electrolyte membrane is prepared by a tape-casting film forming method.
The mechanical properties, mechanical properties and thermal stability of the composite solid electrolyte are improved, the growth of metal dendrites is inhibited, the preparation process is simple, the cost is low, and the electrical conductivity and mechanical strength are significantly improved.
Smart Images

Figure CN112382787B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery manufacturing, and in particular to a composition for forming a composite solid electrolyte, a composite solid electrolyte membrane and a battery comprising the same. Background Art
[0002] In recent years, the rapid expansion of the consumer electronics and electric vehicle markets has driven the development of flexible chemical power sources with high energy density and high safety. Currently, lithium-ion batteries using liquid electrolytes are the most widely used chemical power sources. However, the inherent limitations of non-aqueous liquid electrolytes, such as leakage, high volatility and flammability, seriously affect the safety of lithium-ion batteries, especially at high temperatures, where liquid electrolytes greatly reduce battery safety. In addition, the use of liquid electrolytes in lithium metal batteries can cause the growth of lithium dendrites, and a certain degree of lithium dendrites can pierce the diaphragm and cause safety accidents. Therefore, replacing organic liquid electrolytes with solid polymer electrolytes (SPEs) can alleviate the above safety issues of lithium batteries, and the thinness and flexibility of polymers give electronic devices good processability.
[0003] Polymer electrolytes are composed of a polymer matrix and lithium salts. In solid polymers, ion transport mainly depends on the amorphous phase in the polymer matrix. As the content of the amorphous region increases, the ionic conductivity of the polymer electrolyte will also increase. Therefore, researchers have done a lot of research on lowering the glass transition temperature Tg of the polymer, stabilizing the amorphous region, and increasing the content of the amorphous region. However, the trade-off between ionic conductivity and mechanical strength is a key issue in the design of polymer electrolytes.
[0004] In view of the above problems, it is necessary to provide a solid electrolyte that simultaneously meets the requirements of high ionic conductivity, thermal stability and good mechanical strength. Summary of the invention
[0005] The main purpose of the present invention is to provide a composition for forming a composite solid electrolyte, a composite solid electrolyte membrane and a battery containing the same, so as to solve the problem that the existing solid electrolyte cannot simultaneously meet the requirements of high ionic conductivity, thermal stability and good mechanical strength.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a composition for forming a composite solid electrolyte on the one hand, and the composition for forming a composite solid electrolyte includes: polyurethane and a conductive metal salt, wherein the weight average molecular weight of the polyurethane is 100,000 to 110,000, the hardness is 90 to 100 Shore A, the tensile strength is 35 to 40 MPa, and the conductive metal salt is a lithium salt or a sodium salt.
[0007] Furthermore, in the polyurethane, the solubility of the lithium salt is 0 to 150%.
[0008] Furthermore, the lithium salt is bis(trifluoromethanesulfonyl)imide lithium salt.
[0009] Furthermore, the weight ratio of the polyurethane to the lithium salt is 1:(0.4-1), preferably 1:(0.8-1).
[0010] Furthermore, in polyurethane, the solubility of the sodium salt is 0 to 80%.
[0011] Furthermore, the sodium salt is sodium perchlorate.
[0012] Furthermore, the weight ratio of polyurethane to sodium salt is 1:(0.2-0.8), preferably 1:(0.5-0.7).
[0013] Another aspect of the present application further provides a composite solid electrolyte membrane, which is prepared by using the above composition as a raw material and a tape casting film forming method.
[0014] Furthermore, the thickness of the composite solid electrolyte membrane is 25-50 μm.
[0015] Another aspect of the present application provides a battery, including a solid electrolyte membrane, wherein the solid electrolyte membrane is the composite solid electrolyte membrane provided in the present application.
[0016] By applying the technical scheme of the present invention, the mechanical properties, mechanical properties and thermal stability of the composite solid electrolyte prepared by the above-mentioned composition can be greatly improved by using the polyurethane with the above-mentioned specific molecular weight, hardness and tensile strength as the matrix resin. The composite solid electrolyte prepared by the above-mentioned composition has high ionic conductivity and good mechanical strength, which can effectively inhibit the growth of metal dendrites. At the same time, when preparing the composite solid electrolyte with the above-mentioned composition as the raw material, it is only necessary to dissolve the polyurethane in an organic solvent (such as DMF), add a conductive metal salt and stir and dissolve to obtain a casting liquid, and then obtain a polymer electrolyte after scraping and drying. Therefore, when preparing the composite solid electrolyte with the above-mentioned composition raw material, it has the advantages of simple preparation process, mature production process, no special treatment, low cost, etc. On this basis, the composite solid electrolyte prepared by the above-mentioned composition not only has good mechanical strength, high conductivity and thermal stability, but also has the advantages of simple preparation process, mature production process, low cost, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0018] Figure 1 This is a scanning electron microscope (SEM) image of the SPE-PU membrane prepared in Example 1 of the present application;
[0019] Figure 2 X-ray diffraction analysis (XRD) diagrams of PU, PEO and the SPE-PU film prepared in Example 1;
[0020] Figure 3 This is the linear sweep voltammogram of the SPE-PU membrane prepared in Example 1 of the present application;
[0021] Figure 4 This is the electrochemical impedance diagram of the button cell LiFePO4\SPE-PU\Li prepared in Example 1 of the present application;
[0022] Figure 5 This is a cycle performance diagram of the button cell LiFePO4\SPE-PU\Li prepared in Example 1 of the present application at 0.5C charge and discharge at room temperature;
[0023] Figure 6 The symmetrical lithium battery prepared in Example 1 of the present application is 0.1 mA·cm –2 Potential distribution diagram of repeated lithium plating / stripping under current density;
[0024] Figure 7 This is a scanning electron microscope (SEM) image of the SPE-PU membrane prepared in Example 2 of the present application;
[0025] Figure 8 This is the electrochemical impedance diagram of the button cell Na3V2(PO4)3\SPE-PU\Na prepared in Example 2 of the present application;
[0026] Fig. 9 This is a cycle performance diagram of the button battery Na3V2(PO4)3\SPE-PU\Na prepared in Example 2 of the present application, charged and discharged at 0.5C at room temperature;
[0027] Fig.10 The symmetrical sodium battery prepared in Example 2 of the present application is 0.1 mA·cm –2 Potential distribution under current density. DETAILED DESCRIPTION
[0028] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0029] As described in the background technology, the existing solid electrolytes cannot meet the problems of high ionic conductivity, thermal stability and good mechanical strength at the same time. In order to solve the above technical problems, the present application provides a composition for forming a composite solid electrolyte, and the composition for forming a composite solid electrolyte includes: polyurethane and a conductive metal salt, wherein the weight average molecular weight of the polyurethane is 100,000 to 110,000, the hardness is 90 to 100 Shore A, the tensile strength is 35 to 40 MPa, and the conductive metal salt is a lithium salt or a sodium salt.
[0030] The use of polyurethane with the above-mentioned specific molecular weight, hardness and tensile strength as the matrix resin can greatly improve the mechanical properties, mechanical properties and thermal stability of the composite solid electrolyte prepared by the above-mentioned composition. The composite solid electrolyte prepared by the above-mentioned composition has high ionic conductivity and good mechanical strength, which can effectively inhibit the growth of metal dendrites. At the same time, when preparing the composite solid electrolyte with the above-mentioned composition as the raw material, it is only necessary to dissolve the polyurethane in an organic solvent (such as DMF), add a conductive metal salt and stir and dissolve to obtain a casting liquid, and then obtain a polymer electrolyte after scraping and drying. Therefore, when preparing the composite solid electrolyte with the above-mentioned composition raw material, it has the advantages of simple preparation process, mature production process, no special treatment, and low cost. On this basis, the composite solid electrolyte prepared by the above-mentioned composition not only has good mechanical strength, high conductivity and thermal stability, but also has the advantages of simple preparation process, mature production process, and low cost.
[0031] The lithium salt used in the above-mentioned composition for forming a composite solid electrolyte can be selected from the types commonly used in the art. In a preferred embodiment, the solubility of the lithium salt in polyurethane is 0 to 150%. The solubility of lithium salt in polyurethane is low, which will affect the conductivity in the composite solid electrolyte. Limiting the solubility of lithium salt within the above-mentioned range is beneficial to improving the stability of the electrical properties of the composite solid electrolyte. More preferably, the lithium salt is bistrifluoromethylsulfonyl imide lithium salt. The above-mentioned lithium salt has a large anion radius, which can delocalize the charge of the anion and reduce the lattice energy, thereby improving its solubility in the polymer and the conductivity of the composite solid electrolyte. Therefore, the above-mentioned lithium salt has good stability in the above-mentioned polyurethane matrix resin and can stably coexist with polyurethane.
[0032] In order to further improve the electrical properties of the composite solid electrolyte formed by the above composition, preferably, the weight ratio of polyurethane to lithium salt is 1:(0.4-1), preferably 1:(0.8-1).
[0033] The sodium salt used in the composition for forming the composite solid electrolyte can be selected from the commonly used types in the art. In a preferred embodiment, the solubility of the sodium salt in polyurethane is 0 to 80%. The solubility of the sodium salt in polyurethane is low, which will affect the conductivity in the composite solid electrolyte. Limiting the solubility of the sodium salt within the above range is conducive to improving the stability of the electrical properties of the composite solid electrolyte. More preferably, the sodium salt is sodium perchlorate. The anion radius of the above sodium salt is large, which can delocalize the charge of the anion and reduce the lattice energy, thereby improving its solubility in the polymer and the conductivity of the composite solid electrolyte. Therefore, the above sodium salt has good stability in the above polyurethane matrix resin and can stably coexist with polyurethane.
[0034] In order to further improve the electrical properties of the composite solid electrolyte formed by the above composition, preferably, the weight ratio of polyurethane to sodium salt is 1:(0.2-0.8), preferably 1:(0.5-0.7).
[0035] Another aspect of the present application further provides a composite solid electrolyte membrane, which is prepared by a tape casting method using the composition for forming a composite solid electrolyte provided in the present application as a raw material.
[0036] The polyurethane of the above-mentioned specific molecular weight has a more suitable hardness and tensile property and good heat resistance. Using it as a matrix resin can greatly improve the mechanical properties, mechanical properties and thermal stability of the composite solid electrolyte membrane prepared by the above-mentioned composition. The composite solid electrolyte membrane prepared by the above-mentioned composition has good mechanical strength, which can effectively inhibit the growth of conductive metal salt dendrites, thereby improving the conductivity of the composite solid electrolyte membrane. At the same time, when the composite solid electrolyte membrane is prepared using the above-mentioned composition as a raw material, it is only necessary to melt the polyurethane to obtain a polyurethane melt, and then the conductive metal salt and the above-mentioned polyurethane melt are sequentially mixed and cured. Therefore, when the composite solid electrolyte membrane is prepared using the above-mentioned composition raw material, it has the advantages of simple preparation process, mature production process, no special treatment, and low cost. On this basis, the composite solid electrolyte membrane prepared by the above-mentioned composition not only has good mechanical properties and mechanical properties, as well as high conductivity and thermal stability, but also has the advantages of simple preparation process, mature production process, and low cost.
[0037] Preferably, the thickness of the composite solid electrolyte membrane is 25 to 50 μm. The smaller the thickness of the electrolyte membrane, the smaller the impedance, the better the performance, the smaller the mass and volume, and the more beneficial it is to improve the mass specific capacity and volume specific capacity of the entire battery. However, if the thickness is too small, it is easy to cause local micro-short circuits in the battery during the cycle. Limiting the electrolyte membrane to the above thickness range is beneficial to improving the electrical performance of the composite solid electrolyte membrane and the battery as much as possible while ensuring the normal use of the battery.
[0038] Another aspect of the present application provides a battery, comprising a solid electrolyte membrane, which is the composite solid electrolyte membrane provided in the present application.
[0039] Since the composite solid electrolyte membrane prepared from the above composition not only has good mechanical properties and mechanical properties, high stability, electrical conductivity and thermal stability, but also has the advantages of simple preparation process and low cost, etc., the use of the composite solid electrolyte membrane to prepare lithium-ion batteries or sodium-ion batteries is conducive to further improving the comprehensive performance of the battery such as electrical performance stability and energy density, while reducing its preparation cost.
[0040] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0041] Example 1
[0042] (1) Preparation of composite solid electrolyte membrane (SPE-PU membrane):
[0043] Mix 1g of polyurethane (polyester thermoplastic polyurethane 1190, molecular weight of about 100,000, Wanhua Chemical) with 5.67g of N,N-dimethylformamide (DMF), heat to 60°C and stir until fully dissolved to obtain a 15% solution. Subsequently, the above solution was transferred to a glove box, and 0.8g of bistrifluoromethylsulfonyl imide lithium salt was added and stirred until fully dissolved to obtain a casting liquid. The above casting liquid was evenly scraped onto a glass plate with a small casting machine, and the glass plate was transferred to a 60°C vacuum drying oven and dried for 12 hours. After that, the glass plate was taken out, the PU film was peeled off, and a disc film with a diameter of 18mm was cut with a punching machine and transferred to the glove box for use. The scanning electron microscope image is shown as follows Figure 1 .
[0044] (2) Battery preparation
[0045] Positive electrode preparation:
[0046] Commercial lithium iron phosphate LiFePO4 was used as the positive electrode active material, Super-P (Hefei Kejing Material Technology Co., Ltd.) was used as the conductive agent, and PVDF NMP solution was used as the binder (mixed at a weight ratio of 8:1:1). The dried positive electrode material was ground in an agate mortar for 30 minutes; after grinding evenly, PVDF solution (mass fraction 5%) was added according to the proportion, and stirred on a magnetic stirrer for 6 hours; the obtained paste slurry was evenly coated on the current collector aluminum foil, and then dried in a vacuum drying oven at 60°C for 20 hours before being taken out for use.
[0047] Battery Assembly:
[0048] The dried LiFePO4 electrode is kept under a pressure of 8MPa for 30 to 180s and cut into circular electrodes with a diameter of 12mm by a punching machine to obtain the LiFePO4 positive electrode sheet; metallic lithium with a diameter of 14mm is used as the negative electrode, and the SPE-PU membrane is used as the solid polymer electrolyte. In addition, no liquid electrolyte or additives are added to assemble a CR2032 button battery.
[0049] The lithium symmetric battery uses lithium sheets with a diameter of 12 mm as positive and negative electrodes, SPE-PU as a solid polymer electrolyte, and CR2032 batteries. The entire battery assembly is completed in a glove box.
[0050] (3) Performance test:
[0051] Physical and chemical performance tests:
[0052] XRD was used to test PU, PEO and SPE-PU films. The results are as follows: Figure 2 .from Figure 2 It can be seen that SPE-PU has no obvious crystallinity, and its chain segments have good flexibility and can freely conduct lithium ions. Therefore, SPE-PU has a high ionic conductivity at room temperature.
[0053] The thermal stability of SPE-PU membrane was tested by thermogravimetric analyzer TGA. The results showed that it had good thermal stability and did not decompose within 200℃.
[0054] The glass transition temperature of SPE-PU membrane was tested by DSC. The results showed that it had low crystallinity and high ionic conductivity.
[0055] The mechanical properties of the SPE-PU membrane were tested using a tensile tester. The results showed that it has good mechanical strength and can inhibit lithium dendrites.
[0056] Electrochemical performance test:
[0057] The SPE-PU was subjected to linear voltammetric sweep test using an electrochemical workstation. Figure 3 As shown, it did not decompose below 4.7 V, which indicates its high electrochemical stability.
[0058] Perform impedance test on the battery, such as Figure 4 The results show that SPE-PU has higher room temperature ionic conductivity and better interfacial compatibility.
[0059] The constant current charge and discharge test of lithium iron phosphate battery was carried out using Xinwei battery testing system, and the charge and discharge voltage range was 2.4V to 4.0V. The rate performance test was carried out at 0.1C to 2C rate, and the cycle performance test was carried out at 0.5C rate. The results are as follows Figure 5As shown, curve 1 represents the coulombic efficiency and curve 2 represents the discharge capacity. Figure 5 It can be seen that at a rate of 0.5C, the discharge capacity reaches 130 mAh g -1 After 470 cycles, the capacity did not decay, which shows that the battery has very good cycle performance.
[0060] The charge and discharge test of lithium symmetrical battery was carried out using Xinwei battery testing system at 0.1 mA cm -1 To charge and discharge, Figure 6 , after 400 h, the polarization voltage was still within 0.2 V, confirming that SPE-PU has a certain effect in inhibiting lithium dendrites.
[0061] Example 2
[0062] (1) Preparation of composite solid electrolyte membrane (SPE-PU membrane):
[0063] The sodium salt in Example 1 was replaced with sodium perchlorate, and the mass ratio of polyurethane to sodium perchlorate was 1:0.6, and the sodium metal battery was used. The preparation method and test method were referred to Example 1. Scanning electron microscopy showed Figure 7 .
[0064] (2) Battery preparation
[0065] The sodium vanadium phosphate used for assembling the positive electrode material of the sodium button battery is synthesized as follows:
[0066] Mix 2.52g of citric acid monohydrate, 1.404g of ammonium vanadate, 2.071g of ammonium dihydrogen phosphate and 400g of high-purity water in a 500mL beaker and stir until fully dissolved. Add 0.72g of sodium hydroxide and stir to dissolve, and adjust the pH value to 9 with ammonia water. Put it in a water bath and keep it warm for 12 hours. After the water evaporates completely, transfer the product to a vacuum drying oven and dry it for 12 hours. The dried product is transferred to an agate mortar and ground into powder. It is calcined at 350℃ for 4 hours in a tubular furnace with argon and hydrogen mixed gas (95:5). After cooling naturally, use a high-speed ball mill at 2000r·min –1 Ball milling for 0.5 h, repeated ball milling for 6 times, and then transferred to the tube furnace again, heated to 800 ° C in argon atmosphere, kept warm for 8 h, cooled naturally, and then used a high-speed ball mill at 2000 r / min –1 Ball milling was performed for 0.5 h and repeated 6 times to obtain the powdered positive electrode material Na3V2(PO4)3.
[0067] The preparation method of Na3V2(PO4)3 positive electrode sheet refers to the preparation method of LiFePO4 positive electrode sheet in Example 1.
[0068] (3)Performance testing.
[0069] Physical and chemical performance tests:
[0070] The thermal stability of SPE-PU membrane was tested by thermogravimetric analyzer TGA. The results showed that it had good thermal stability and did not decompose within 200℃.
[0071] The glass transition temperature of SPE-PU membrane was tested by DSC. The results showed that it had low crystallinity and high ionic conductivity.
[0072] The mechanical properties of SPE-PU membrane were tested by tensile tester. The results showed that it has good mechanical strength and can inhibit sodium dendrites.
[0073] Electrochemical performance test:
[0074] Perform impedance test on the battery, such as Figure 8 The results show that SPE-PU has higher room temperature ionic conductivity and better interfacial compatibility.
[0075] The constant current charge and discharge test of sodium iron phosphate battery was carried out using Xinwei battery testing system. The test results are as follows Fig. 9 , where curve A represents the coulombic efficiency and curve B represents the discharge capacity. Fig. 9 It can be seen that the sodium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 370 cycles at room temperature and 0.5C rate, and the discharge capacity reaches 75mAh·g -1 , the Coulomb efficiency basically remains above 99%.
[0076] The sodium symmetric battery was charged and discharged using the Xinwei battery testing system at 0.1 mA cm -1 To charge and discharge, Fig.10 , after 300 h, the polarization voltage was still within 0.2 V, confirming that SPE-PU has a certain effect in inhibiting sodium dendrites.
[0077] Example 3
[0078] The difference from Example 1 is that the weight ratio of polyurethane to lithium salt is 1:0.6.
[0079] The lithium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 430 cycles at room temperature and 0.5C rate, with a discharge capacity of 127mAh·g -1 , the Coulomb efficiency basically remains above 99%.
[0080] The battery was tested for charge and discharge using the Xinwei battery testing system at 0.1 mA cm -1 After charging and discharging, the polarization voltage was still within 0.2 V after 400 h, which confirmed that SPE-PU has a certain effect in inhibiting lithium dendrites.
[0081] Example 4
[0082] The difference from Example 1 is that the weight ratio of polyurethane to lithium salt is 1:0.2.
[0083] The lithium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 200 cycles at room temperature and 0.5C rate, with a discharge capacity of 122mAh·g -1 , the Coulomb efficiency basically remains above 98%.
[0084] The battery was tested for charge and discharge using the Xinwei battery testing system at 0.1 mA cm -1 After charge and discharge, the polarization voltage was still within 0.2V after 300h, which confirmed that SPE-PU has a certain effect in inhibiting lithium dendrites.
[0085] Example 5
[0086] The difference from Example 1 is that the lithium salt is lithium hexafluorophosphate (LiPF6).
[0087] The lithium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 380 cycles at room temperature and 0.5C rate, with a discharge capacity of 118mAh·g -1 , the Coulomb efficiency basically remains above 97%.
[0088] The battery was tested for charge and discharge using the Xinwei battery testing system at 0.1 mA cm -1 After charge and discharge, the polarization voltage was still within 0.2V after 300h, which confirmed that SPE-PU has a certain effect in inhibiting lithium dendrites.
[0089] Example 6
[0090] The difference from Example 2 is that the weight ratio of polyurethane to sodium salt is 1:0.5.
[0091] The sodium vanadium phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 300 cycles at room temperature and 0.5C rate, with a discharge capacity of 75mAh·g -1 , the Coulomb efficiency basically remains above 98%.
[0092] The sodium symmetric battery was charged and discharged using the Xinwei battery testing system at 0.1 mA cm -1 After charge and discharge, the polarization voltage was still within 0.2 V after 300 h, which confirmed that SPE-PU had a certain effect in inhibiting sodium dendrites.
[0093] Example 7
[0094] The difference from Example 2 is that the weight ratio of polyurethane to sodium salt is 1:0.3.
[0095] The sodium vanadium phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 300 cycles at room temperature and 0.5C rate, with a discharge capacity of 67.mAh·g -1 , the Coulomb efficiency basically remains above 97%.
[0096] The sodium symmetric battery was charged and discharged using the Xinwei battery testing system at 0.1 mA cm -1 After charge and discharge, the polarization voltage was still within 0.2 V after 287 h, which confirmed that SPE-PU had a certain effect in inhibiting sodium dendrites.
[0097] Example 8
[0098] The difference from Example 2 is that the sodium salt is sodium bis(trifluoromethylsulfonyl)imide.
[0099] The sodium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 300 cycles at room temperature and 0.5C rate, with a discharge capacity of 65mAh g -1 , the Coulomb efficiency basically remains above 95%.
[0100] The sodium symmetric battery was charged and discharged using the Xinwei battery testing system at 0.1 mA cm -1 After charge and discharge, the polarization voltage was still within 0.2 V after 260 h, which confirmed that SPE-PU had a certain effect in inhibiting sodium dendrites.
[0101] Comparative Example 1
[0102] The difference from Example 1 is:
[0103] The weight average molecular weight of polyether thermoplastic polyurethane 8190 is 110,000, the hardness is 90 Shore A, and the tensile strength is 28 MPa. It comes from Wanhua Chemical.
[0104] The lithium iron phosphate battery with SPE-PU as electrolyte can maintain a relatively stable discharge capacity after 150 cycles at room temperature and 0.5C rate, with a discharge capacity of 116.mAh·g -1 , the Coulomb efficiency basically remains above 95%.
[0105] The battery was tested for charge and discharge using the Xinwei battery testing system at 0.1 mA cm -1 After charging and discharging, the polarization voltage was still within 0.2V after 200h, which confirmed that SPE-PU has a certain effect in inhibiting lithium dendrites.
[0106] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0107] By comparing Examples 1 to 8 and Comparative Example 1, it can be seen that the solid electrolyte formed by using the composition provided in the present application can greatly improve its ionic conductivity, thermal stability and mechanical strength.
[0108] By comparing Examples 1, 3, 4 and 5, it can be seen that limiting the weight ratio of polyurethane to lithium salt within the preferred range of the present application and selecting a composition of the preferred lithium salt type of the present application to form a solid electrolyte can greatly improve its ionic conductivity, thermal stability and mechanical strength.
[0109] By comparing Examples 2, 6 to 8, it can be seen that limiting the weight ratio of polyurethane to sodium salt within the preferred range of the present application and selecting the preferred sodium salt type composition of the present application to form a solid electrolyte can greatly improve its ionic conductivity, thermal stability and mechanical strength.
[0110] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composition for forming a composite solid electrolyte, characterized in that: The composition for forming a composite solid electrolyte comprises: polyurethane and a conductive metal salt, wherein the weight average molecular weight of the polyurethane is 100,000 to 110,000, the hardness is 90 to 100 Shore A, and the tensile strength is 35 to 40 MPa, and the conductive metal salt is a lithium salt or a sodium salt; the weight ratio of the polyurethane to the lithium salt is 1:(0.4 to 0.8); the weight ratio of the polyurethane to the sodium salt is 1:(0.5 to 0.7); the lithium salt is bistrifluoromethylsulfonyl imide lithium salt, and the sodium salt is sodium perchlorate salt.
2. The composition for forming a composite solid electrolyte according to claim 1, characterized in that: In the polyurethane, the solubility of the lithium salt is 0 to 150%.
3. The composition for forming a composite solid electrolyte according to claim 1, characterized in that: In the polyurethane, the solubility of the sodium salt is 0 to 80%.
4. A composite solid electrolyte membrane, characterized in that: The composite solid electrolyte membrane is prepared by using the composition according to any one of claims 1 to 3 as a raw material and adopting a tape casting film forming method.
5. The composite solid electrolyte membrane according to claim 4, characterized in that: The thickness of the composite solid electrolyte membrane is 25-50 μm.
6. A battery comprising a solid electrolyte membrane, characterized in that: The solid electrolyte membrane is the composite solid electrolyte membrane according to claim 4 or 5.