Thin film formation method

By supplying heated oxidation gas and silicon source gas to the treated body at low temperature to form a silicon oxide film, the problems of thin film formation and roughness improvement at low temperature are solved, and film formation and surface are achieved at a temperature below 400°C Reduced roughness.

CN112703580BActive Publication Date: 2024-12-03EUGENE TECH CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN201980058805.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-11
Filing Date
2019-09-09
Publication Date
2024-12-03
Estimated Expiration
2039-09-09

AI Technical Summary

Technical Problem

The prior art is difficult to effectively form a thin film at a low temperature below 400°C, and the surface roughness of the film is high, affecting process performance.

Method used

By supplying the treated body with an oxidation gas and a silicon source gas heated at more than 400°C in the chamber, a silicon oxide film is formed. The oxidation gas is supplied in a thermally decomposed state after cooling, and combined with appropriate chamber pressure and gas flow rate, a silicon oxide film is formed Low roughness silicon oxide film.

Benefits of technology

The film is formed at a temperature below 400°C, and the surface roughness of the film is significantly reduced to less than 1.0, improving the flatness and process performance of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112703580B_ABST
    Figure CN112703580B_ABST
Patent Text Reader

Abstract

According to one embodiment of the present invention, a thin film forming method loads a processed object into a chamber, controls the temperature of the processed object to be below 400°C, and supplies silicon source gas and oxidizing gas into the chamber to form a silicon oxide film on the surface of the processed object, characterized in that the oxidizing gas is heated to a temperature exceeding 400°C before being supplied into the chamber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for forming a thin film, and more particularly to a method capable of forming a thin film at a low temperature. Background Art

[0002] In recent years, there has been a demand for thin films formed at low temperatures, and thin films formed at extremely low temperatures below 400° C. have been studied. In particular, it is desired to provide a thin film forming process capable of improving the average roughness of a thin film by the process compared with existing processes. Summary of the invention

[0003] Issues to be solved

[0004] An object of the present invention is to provide a method capable of forming a thin film at a low temperature.

[0005] Another object of the present invention is to provide a method for forming a thin film that can improve the surface roughness of the thin film.

[0006] Other objects of the present invention will become more apparent from the following detailed description and accompanying drawings.

[0007] Problem Solution

[0008] According to one embodiment of the present invention, a thin film forming method is provided, wherein a processed object is loaded into a chamber, the temperature of the processed object is controlled to be below 400°C, and a silicon source gas and an oxidizing gas are supplied into the chamber to form a silicon oxide film on the surface of the processed object, wherein the oxidizing gas is heated to a temperature exceeding 400°C before being supplied into the chamber.

[0009] The oxidizing gas may be supplied into the chamber after being cooled to a temperature lower than a temperature of the object to be processed in a thermally decomposed state.

[0010] The oxidizing gas may be heated to 700-900°C.

[0011] The oxidizing gas may be N 2 O or O 2 , and the flow rate of the above-mentioned oxidizing gas supplied into the above-mentioned chamber can be 3000-7000 SCCM.

[0012] The silicon source gas may be silane or disilane, and the flow rate of the oxidizing gas supplied into the chamber may be 50-100 SCCM.

[0013] The pressure inside the chamber may be 25-150 Torr.

[0014] The above method may further include the step of forming an upper thin film on the upper portion of the above silicon oxide film, and the above upper thin film may be any one of an amorphous silicon thin film doped with boron (B), an undoped amorphous silicon thin film and an amorphous silicon thin film doped with phosphorus (P).

[0015] The thickness of the silicon oxide film may be

[0016] The method may further include forming an underlayer before forming the silicon oxide film, and forming the silicon oxide film on the underlayer. The underlayer may be any one of a thermal oxide film, a silicon nitride film and an amorphous carbon film.

[0017] According to one embodiment of the present invention, a thin film forming device for forming a silicon oxide film includes: a chamber having an internal space blocked from the outside, and performing a process in the above-mentioned internal space; a susceptor, which is arranged in the above-mentioned chamber, on which a processed object is placed, and has a built-in heater; a silicon source gas supplier, which is used to store silicon source gas; an oxidation gas source supplier, which is used to store oxidation gas; a carrier gas supplier, which is used to store carrier gas; a silicon source supply line, which is connected to the above-mentioned silicon source gas supplier to supply the above-mentioned silicon source gas into the above-mentioned chamber; a carrier gas supply line, which is connected to the above-mentioned carrier gas supplier to supply the carrier gas into the above-mentioned chamber; a main supply line, which is connected to the above-mentioned silicon source supply line and the above-mentioned carrier gas supply line in a state of being connected to the above-mentioned chamber; an oxidation gas supply line, which is connected to the above-mentioned main supply line and connected to the above-mentioned oxidation gas source supplier to supply the above-mentioned oxidation gas into the above-mentioned chamber; and an oxidation gas heater, which is arranged on the above-mentioned oxidation gas supply line and heats the above-mentioned oxidation gas to a temperature exceeding 400°C.

[0018] Effects of the Invention

[0019] According to an embodiment of the present invention, a thin film can be formed at a temperature below 400° C. In addition, the surface roughness of the thin film can be reduced to less than 1.0. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 FIG. 1 is a view schematically showing a thin film forming apparatus according to an embodiment of the present invention.

[0021] Figure 2 and Figure 3 This is a graph showing the film formation rate according to the temperature of the object to be processed when the oxidizing gas is supplied after being heated and when the oxidizing gas is supplied after being not heated.

[0022] Figure 4 is a graph showing the average roughness of thin films for the same underlying film.

[0023] Figure 5 The figure shows the average roughness of the thin film for various base films.

[0024] Figure 6 This is a graph showing the average roughness of the film according to the thickness of the silicon oxide film.

[0025] Figure 7 This is a graph showing the average roughness of the thin film according to the temperature of the processed object.

[0026] Figure 8 This is a graph showing the film formation rate according to the heating temperature of the oxidizing gas for various temperatures of the processed objects.

[0027] Fig. 9 It is a graph which shows the film formation rate according to the flow rate of an oxidizing gas.

[0028] Fig.10 It is a graph showing the film forming rate according to the processing pressure.

[0029] Fig.11 The graph shows the film formation rate according to the flow rate of the silicon source gas. DETAILED DESCRIPTION

[0030] Below, refer to the attached Figures 1 to 11 The preferred embodiment of the present invention is described in more detail. The embodiment of the present invention can be deformed into various forms, and the scope of the present invention should not be interpreted as being limited to the embodiment described below. This embodiment is provided to explain the present invention in more detail to a person skilled in the art of the present invention. Therefore, in order to emphasize a clearer description, the shapes of the elements appearing in the drawings may be exaggerated.

[0031] Figure 1 The figure schematically shows a thin film forming apparatus according to an embodiment of the present invention. The thin film forming apparatus has a chamber blocked from the outside, a base is provided in the chamber, and a processed object (or substrate) is placed on the base. When the processed object is placed on the base, a thin film is formed on the surface of the processed object, and the base can heat the processed object to the necessary process temperature through a built-in heater.

[0032] As the silicon source (Si source) gas, silane or disilane (or other silicon source gases) can be selected as needed; nitrogen (N 2 ) can be used as a carrier gas. The silicon source gas supplier and the carrier gas supplier can be connected to a main supply line connected to the chamber and supplied to the chamber together.

[0033] As the oxidizing gas, nitrogen oxide (N 2 O), oxygen (O 2 ) or H 2 O. The oxidizing gas supplier may be connected to a supply line connected to the chamber and supplied to the chamber. In this case, a line heater may be provided on the supply line, and the oxidizing gas may be supplied to the chamber in a state where the oxidizing gas is heated to a necessary process temperature by the line heater. Since the line heater is a known technology, a detailed description thereof is omitted.

[0034] pass Figure 1 A method for forming a silicon oxide film is described. The object to be processed is adjusted to a necessary process temperature / pressure while being placed on a susceptor in a chamber. The process temperature can be adjusted by a heater provided on the susceptor, and the process pressure can be adjusted by an exhaust line / pump (not shown) connected to the chamber. The process temperature can be below 400°C.

[0035] The silicon source gas and the carrier gas are supplied through the main supply line, and the oxidizing gas is supplied through the supply line. At this time, the silicon source gas and the carrier gas are supplied at room temperature, while the oxidizing gas is supplied in a state heated by the line heater.

[0036] The line heater heats the oxidizing gas to a temperature above the thermal decomposition temperature, so the oxidizing gas is supplied to the interior of the chamber in a state of being thermally decomposed. The oxidizing gas is naturally cooled before being supplied to the interior of the chamber, and the chamber adopts a cold wall type. Therefore, the temperature of the oxidizing gas supplied to the interior of the chamber can be lower than 100°C, but since the oxidizing gas maintains a thermally decomposed state, it will not have any effect on the formation of the silicon oxide film. In addition, when the temperature of the oxidizing gas is higher than the temperature of the processed object (or substrate), it may affect the underlying film formed on the processed object. Therefore, the temperature of the oxidizing gas should be lower than the temperature of the processed object (for example, 400°C). In this way, a silicon oxide film can be formed even when the temperature of the processed object is below 400°C.

[0037] Figure 2 and Figure 3 This is a graph showing the film formation rate according to the temperature of the object to be processed when the oxidizing gas is supplied after being heated and when the oxidizing gas is supplied after being not heated. Figure 2As shown in the figure, when the temperature inside the chamber (or the temperature of the object to be processed) is 300-400°C, if an unheated oxidizing gas is supplied, a silicon oxide film is not formed at all. On the other hand, when an oxidizing gas heated by a line heater is supplied, a silicon oxide film is formed even when the temperature of the object to be processed is below 400°C, and the film formation rate (D / R) is 1.57 at 300°C. Therefore, it can be seen that a silicon oxide film is formed even if the process temperature of the silicon oxide film (or the temperature of the object to be processed) is lowered to 300°C. In particular, it can be seen that the film formation rate increases approximately linearly with the process temperature.

[0038] In addition, if Figure 3 As shown in FIG. 1 , when the temperature of the object to be processed is 300-350°C, if an unheated oxidizing gas is supplied, a silicon oxide film is not formed at all. On the other hand, when an oxidizing gas heated by a line heater is supplied, a silicon oxide film is formed even if the temperature of the object to be processed is below 400°C. 4 ) case, at 300°C, the film formation ratio (D / R) also showed 0.07; in disilane (Si 2 H 6 ), the film formation rate (D / R) also showed 1.66 at 310°C. Therefore, it can be seen that even if the process temperature of the silicon oxide film (or the temperature of the processed object) is lowered to below 350°C, the silicon oxide film will be formed. In particular, it can be seen that the film formation rate increases approximately linearly with the processing temperature.

[0039] Figure 4 This is a graph showing the average roughness of thin films for the same base film. After the thermal oxidation film is formed, the oxidizing gas is heated and supplied as described above, and the oxidizing gas is deposited at a temperature below 400°C. After forming a silicon oxide film (LTO) and then forming multiple upper films on it, the average roughness of the upper films is significantly improved.

[0040] Specifically, at 300°C, when a low-temperature boron-doped amorphous silicon film is deposited on the top of the underlying film, if a silicon oxide film (LTO) is deposited, the average roughness is improved from 1.011 to 0.475. In addition, at 500°C, when an undoped amorphous silicon film is deposited on the top of the underlying film, if a silicon oxide film (LTO) is deposited, the average roughness is improved from 0.536 to 0.244. In addition, at 500°C, when an amorphous silicon film doped with phosphorus is deposited on the top of the underlying film, if a silicon oxide film (LTO) is deposited, the average roughness is improved from 0.589 to 0.255.

[0041] Figure 5The graph shows the average roughness of the thin film for various base films. It is known that the various base films were deposited at a temperature lower than 400°C by supplying heated oxidizing gas. When a low-temperature boron-doped amorphous silicon film is formed on top of a LTO film at 300°C, the average roughness of the upper film is significantly improved.

[0042] Specifically, when a low-temperature boron-doped amorphous silicon film is deposited on a (bare) target object without a thin film, the average roughness is improved from 0.978 to 0.442 when a silicon oxide film (LTO) is deposited. In the case of depositing a low temperature boron-doped amorphous silicon film on the thermal oxide film, if a silicon oxide film (LTO) is deposited, the average roughness is improved from 1.011 to 0.475. In the case of depositing a low temperature boron-doped amorphous silicon film on the nitride film, if a silicon oxide film (LTO) is deposited, the average roughness is improved from 0.809 to 0.733. In the case where a silicon film doped with boron at a low temperature is deposited on the amorphous carbon film (ACL), if the silicon oxide film (LTO) is deposited, the average roughness is improved from 0.826 to 0.631.

[0043] Figure 6 This is a graph showing the average roughness of the film according to the thickness of the silicon oxide film. Figure 6 As shown, it can be seen that when an amorphous silicon film doped with boron at a low temperature is deposited on a (bare) processing body without a thin film formed thereon, the average roughness is improved as the thickness of the silicon oxide film (LTO) increases.

[0044] Figure 7 This is a graph showing the average roughness of the thin film according to the temperature of the treated object. Figure 7 As shown in FIG. 1 , when a low-temperature boron-doped amorphous silicon film is deposited on a (bare) object to be processed without a thin film, the average roughness varies depending on the process temperature (or the temperature of the object to be processed). Specifically, when the process temperature (or the temperature of the object to be processed) is 300°C, when disilane is used to form the amorphous silicon film, the average roughness varies depending on the process temperature (or the temperature of the object to be processed). When the silicon oxide film (LTO) is formed, the average roughness is improved from 0.978 to 0.442. In addition, when the process temperature (or the temperature of the processed object) is 600°C, when disilane is used to form When the silicon oxide film (LTO) is formed by using monosilane, the average roughness is improved to 0.534, and when the process temperature (or the temperature of the processed object) is 600°C, When the silicon oxide film (LTO) is used, the average roughness is improved to 0.493.

[0045] Figure 8 This is a graph showing the film formation rate according to the heating temperature of the oxidizing gas for various temperatures of the processed objects. Figure 8 As shown in the figure, it can be seen that when the oxidizing gas is supplied after being heated to 900°C, the film formation rate according to the process temperature (or the temperature of the object to be processed) increases. In addition, it can be seen that when the process temperature is set to 400°C, the film formation rate decreases as the heating temperature of the oxidizing gas decreases. This is believed to be caused by the decrease in the degree of thermal decomposition of the oxidizing gas when the heating temperature of the oxidizing gas decreases.

[0046] Fig. 9 This is a graph showing the film formation rate according to the flow rate of the oxidizing gas. Fig. 9 As shown, when the flow rate of the oxidizing gas is lower than 6000 SCCM, the film forming rate is extremely small. Therefore, it is preferred that the flow rate of the oxidizing gas is higher than 6000 SCCM.

[0047] Fig.10 This is a graph showing the film formation rate according to the processing pressure. Fig.10 As shown, when the process pressure inside the chamber is 50-100 Torr, the film forming rate is high, and therefore, the process pressure is preferably 50-100 Torr, but may be 25 to 150 Torr as needed.

[0048] Fig.11 This is a graph showing the film formation rate according to the flow rate of the silicon source gas. Fig.11 As shown, when the flow rate of disilane is lower than 70 SCCM, the film forming rate is extremely small, therefore, the flow rate of disilane is preferably 70-100 SCCM.

[0049] On the one hand, in this embodiment, the silicon oxide film is formed by supplying the oxidizing gas after heating. However, in the same manner, a nitriding gas (e.g., NH 3 ) to form a silicon nitride film.

[0050] Although the present invention has been described in detail with reference to the preferred embodiments, other embodiments are possible. Therefore, the technical concept and scope of the claims described below are not limited to the preferred embodiments.

[0051] Industrial Applicability

[0052] The present invention can be applied to various forms of semiconductor manufacturing equipment and manufacturing methods.

Claims

1. A method for forming a thin film, It is characterized in that include: The step of loading the object to be processed into the chamber and controlling the temperature of the object to be processed to be below 400° C.; and supplying a silicon source gas and an oxidizing gas into the chamber through a main supply line connected to the chamber to form a silicon oxide film on the surface of the object to be processed, The oxidizing gas is heated to a temperature exceeding 400°C before being supplied into the chamber to become a thermally decomposed state, and then mixed with the silicon source gas and the carrier gas at room temperature in the main supply line, so that the oxidizing gas is cooled by the silicon source gas and the carrier gas in the main supply line and then supplied into the chamber in a thermally decomposed state at a temperature lower than the temperature of the processed object.

2. The thin film forming method according to claim 1, It is characterized in that The above oxidizing gas is heated to 700-900°C.

3. The thin film forming method according to claim 1, It is characterized in that The above oxidizing gas is N 2 O or O 2 , and the flow rate of the above-mentioned oxidizing gas supplied into the above-mentioned chamber is 3000-7000 SCCM.

4. The thin film forming method according to claim 1, It is characterized in that The silicon source gas is silane or disilane, and the flow rate of the silicon source gas supplied into the chamber is 50-100 SCCM.

5. The thin film forming method according to claim 1, It is characterized in that The pressure inside the chamber is 25-150 Torr.

6. The thin film forming method according to claim 1, It is characterized in that The above-mentioned thin film forming method further includes the step of forming an upper thin film on the upper part of the above-mentioned silicon oxide film, and the above-mentioned upper thin film is any one of an amorphous silicon film doped with boron (B), an undoped amorphous silicon film and an amorphous silicon film doped with phosphorus (P).

7. The thin film forming method according to claim 6, It is characterized in that The thickness of the silicon oxide film is 8. The thin film forming method according to claim 1, It is characterized in that The thin film forming method further comprises: forming an underlying film before forming the silicon oxide film, and then forming the silicon oxide film on the upper part of the underlying film; The above-mentioned underlying film is any one of a thermal oxide film, a silicon nitride film and an amorphous carbon film.

Citation Information

Patent Citations

  • Film forming method of silicon oxide film, silicon oxide film, semiconductor device, and manufacturing method of semicomductor device

    CN102027580A

  • Film formation method and film formation apparatus

    CN102242350A

  • Advanced process flow for high quality fcvd films

    CN107109643A

  • System for depositing a film onto a substrate using a low vapor pressure gas precursor

    CN1662674A

  • Reduced leakage antifuse structure and fabrication method

    KR100230158B1