A method for enriching magnesium-containing minerals in asbestos tailings

By combining crushing, grinding, flotation and magnetic separation processes, the problem of separating and enriching magnesium-containing minerals in asbestos tailings has been solved, improving the grade of magnesium ore and reducing the aluminum content. This method is suitable for the production of magnesium silicate gel and building materials.

CN113083496BActive Publication Date: 2024-11-12CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110362892.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-02
Publication Date
2024-11-12
Estimated Expiration
2041-04-02

AI Technical Summary

Technical Problem

Existing technologies for separating and enriching magnesium-containing minerals in asbestos tailings suffer from problems such as complex mineral composition, numerous harmful components, difficulty in leaching, low product purity, and high cost. In particular, it is difficult to effectively remove minerals such as quartz and feldspar after pre-enrichment.

Method used

By combining crushing, grinding, flotation and magnetic separation processes, the particle size of the minerals is controlled and flotation is performed using modified carboxylated starch and amphoteric collectors. Subsequently, magnetic separation is carried out to separate magnesium-containing minerals and improve their grade.

Benefits of technology

It achieves efficient enrichment of magnesium-containing minerals in asbestos tailings, increasing MgO content to over 43% and reducing Al2O3 content to below 1.7%, making it suitable for use in magnesium silicate gel and magnesium oxide chemical leaching. Magnetite can be used in building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113083496B_ABST
    Figure CN113083496B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for enriching magnesium-containing minerals in asbestos tailings, which is characterized by: (1) crushing or grinding the asbestos tailings to control the dissociation particle size to be -0.71 mm; (2) controlling the classification cutting particle size to be 0.105 mm-0.038 mm, and classifying the crushed or ground asbestos tailings to obtain fine-grained asbestos tailings and coarse-grained asbestos tailings; flotation of the coarse-grained asbestos tailings, wherein the inhibitor is modified carboxyl starch, and the collector and frother is an amphoteric collector or a cationic collector; (3) grinding the fine-grained asbestos tailings obtained by classification and the flotation concentrate together to obtain minerals with a particle size of -0.105 mm; and magnetic separation is performed to control the magnetic field strength to be ≤4000 Gs to obtain magnetite and magnesium-containing minerals. Beneficial effects: The process is simple and suitable for industrial production; through the combined process, magnesium-containing minerals in co-existing asbestos tailings such as serpentine, quartz, feldspar, and magnetite can be effectively extracted to achieve aluminum reduction, quartz removal, and improve the grade of magnesium-containing minerals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral processing and relates to a method for enriching magnesium-containing minerals in asbestos tailings. Background Art

[0002] Asbestos tailings are the mineral residues left over from asbestos mining. The main mineral components include serpentine, chrysotile, quartz, feldspar, magnetite, calcite, brucite, etc. The main chemical components include MgO, SiO2, Al2O3, Fe2O3, etc. The asbestos content in my country's asbestos mines is usually no more than 5%, so the current reserves of asbestos tailings in my country are about hundreds of millions of tons.

[0003] At present, there are two main comprehensive utilization plans for asbestos tailings:

[0004] One solution is to use the whole mixture to produce concrete aggregate, microcrystalline glass, refractory materials, thermal insulation materials, etc. For example, China Patent (CN104152686A) describes a method for decomposing asbestos tailings, which directly performs mechanical activation, multi-stage acid hydrolysis, washing, alkaline hydrolysis and other process methods on the asbestos tailings to obtain silicon powder, water glass, etc.; China Patent (CN104891951A) describes a method for extracting silicon, magnesium, and aluminum composite thermal insulation materials from asbestos tailings, which directly grinds the asbestos tailings into powder, activates them, and uses chemical leaching methods to obtain silicon, magnesium, aluminum and other elements, thereby obtaining thermal insulation composite materials; China Patent (CN109320089A) describes a functional microcrystalline glass using asbestos tailings as raw materials, in which the mass proportion of asbestos tailings in the raw materials is 90% to 100%.

[0005] Another scheme is to pretreat the minerals first, sort some of the minerals and then use them separately. For example, a Chinese patent (CN111393127A) mentions a method for preparing silica-magnesium gel from iron ore concentrate and residues of asbestos tailings by magnetic separation. The asbestos tailings are crushed, ground and sieved, mixed and ground with alkali and carbon-containing materials, and then roasted and activated to obtain an activated residue; the activated residue is magnetically separated to obtain iron ore concentrate and silica-magnesium residue; the silica-magnesium residue is impregnated with alkali solution and filtered to obtain an alkali leaching solution and an alkali leaching residue; the alkali leaching solution is adjusted to a pH value of 3-5 with acid solution, CO2 is introduced to obtain silica colloid, the alkali leaching residue is dissolved with acid solution to obtain a magnesium salt solution, and CO2 is introduced to obtain a magnesium bicarbonate solution; the silica colloid and the magnesium bicarbonate solution are mixed, an organic foaming agent and a curing agent are added, the mixture is stirred and evaporated to obtain silica-magnesium gel. A Chinese patent (CN111410576A) discloses a method for detoxifying and recycling asbestos tailings by an activation-co-reduction method. The method includes grinding the asbestos tailings into powder and then subjecting them to preliminary magnetic separation to obtain iron concentrate 1 and treated asbestos tailings powder; uniformly mixing the treated asbestos tailings powder with a reducing agent and an activating agent, heating the mixture to 100-300°C under an inert atmosphere for activation / reduction reaction to obtain an activated calcined product; and then subjecting the activated calcined product to secondary magnetic separation to obtain iron concentrate 2 and a detoxified residue.

[0006] Because the mineral composition of asbestos tailings is relatively complex (usually containing at least two or more different types of minerals), the first method uses the asbestos tailings as a whole, and when it is directly used to manufacture building materials, it often contains more harmful mineral components; when the useful components are directly leached to extract the whole components, it often contains more heavy metals or harmful components, which makes it difficult to separate the different useful components after leaching, the product purity is low and the production cost is high (the consumption of leaching aids is large, and the side reactions in the chemical leaching process are many and complex); in the second method, although the quartz and long-grained ore are removed in advance by the mineral processing method, the ore is not removed in advance by the mineral processing method. The separation and enrichment of magnesium-containing minerals from asbestos tailings is rarely reported. Summary of the invention

[0007] The purpose of the present invention is to solve the problem that it is difficult to separate quartz, feldspar and other minerals from the pre-enriched magnesium ore after pre-removing quartz, feldspar and other minerals in the existing ore dressing method, and the grade of the magnesium-containing minerals is not high, and to provide a method for enriching magnesium-containing minerals in asbestos tailings.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for enriching magnesium-containing minerals in asbestos tailings, characterized by comprising the following steps:

[0010] (1) directly crush or grind the asbestos tailings (including serpentine, chrysotile, magnetite, quartz, feldspar and a small amount of dolomite, calcite, brucite and other minerals) to control the dissociation particle size of the minerals to -0.71mm and at the same time control the particle size to be not less than the lower limit of flotation (0.105mm);

[0011] Due to the co-existence of different minerals in asbestos tailings, crushing or grinding the asbestos tailings can dissociate the different minerals in the asbestos tailings and control the dissociation particle size of the minerals at -0.71mm. This is mainly based on the following considerations: 1. To ensure that quartz, feldspar, serpentine, magnetite and other minerals are fully dissociated from each other, which is conducive to mineral separation; 2. To meet the upper limit of the particle size separation by flotation method, to prevent the mineral particles from being too large and causing the flotation process to "sink", making the flotation process impossible; at the same time, the mineral particle size is controlled to be not less than the lower limit of flotation, mainly to improve the efficiency of subsequent flotation. If the mineral particle size is too small, the selectivity of the flotation agent for the target mineral will be reduced;

[0012] (2) Control the graded cutting particle size to 0.105mm~0.038mm, and classify the crushed or ground asbestos tailings to obtain fine-grained asbestos tailings and coarse-grained asbestos tailings; the coarse-grained asbestos tailings are floated by quartz and feldspar mixed flotation method, wherein the inhibitor is modified carboxyl starch (the usage amount is not higher than 1.0kg / t), the collector and frother is an amphoteric collector or a cationic collector (the usage amount is determined according to the content of quartz and feldspar, generally not higher than 1.5kg / t), the flotation foam is the flotation tailings (the main components are quartz, feldspar and the intergrowths and inclusions of the two with serpentine and magnetite), and the sediment is the flotation concentrate (the main components are magnesium-containing minerals and magnetite intergrowths and inclusions);

[0013] Since the hardness of magnesium-containing minerals such as serpentine and brucite is lower than that of quartz and feldspar, some over-crushed magnesium-containing minerals such as serpentine and brucite will enter the fine-grained asbestos tailings through classification. After classification, the particle size composition of coarse-grained asbestos tailings is obtained: the content of graded cutting particle size to 0.71mm accounts for 95% or more of the whole particle size;

[0014] (3) Grinding the fine-grained asbestos tailings and flotation concentrate obtained by classification in step (2) together to obtain minerals (containing magnesium minerals) with a particle size of -0.105 mm; then subjecting the minerals to magnetic separation, controlling the magnetic field strength to no more than 4000 Gs, to obtain magnetite (or a combination or inclusion of magnetite and serpentine) and magnesium-containing minerals (serpentine).

[0015] Furthermore, the classification in step (2) is hydraulic classification, airflow classification or dry and wet screening.

[0016] Furthermore, in the step (2), the flotation concentrate is subjected to one or more scavenging steps.

[0017] Furthermore, the fine-grained asbestos tailings and flotation concentrate obtained by classification in step (2) are directly subjected to magnetic separation (without grinding).

[0018] Furthermore, the magnetite and magnesium-containing minerals after magnetic separation in step (3) are re-grinded and re-magnetically separated.

[0019] Furthermore, the main components of the magnetite after magnetic separation in step (3) are monomer magnetite or a combination of magnetite and magnesium-containing minerals such as serpentine, and the Fe2O3 content is not less than 8%. The main component of the magnesium-containing mineral is serpentine, and its MgO content is increased by 2.2% compared with the selected original ore (asbestos tailings).

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The process steps of the present invention are simple, easy to operate, and suitable for industrial production and application;

[0022] (2) The present invention can effectively extract magnesium-containing minerals in co-existing asbestos tailings such as serpentine, quartz, feldspar, and magnetite by combining crushing, grinding, flotation, and magnetic separation processes on asbestos tailings, thereby achieving the purpose of reducing aluminum (the Al2O3 content is reduced to less than 1.7%) and removing quartz (quartz is enriched in flotation tailings, and serpentine minerals contain SiO2, so the MgO content in the flotation serpentine concentrate increases, and the SiO2 content increases simultaneously, but the SiO2 and Al2O3 contents in the flotation tailings increase, which indirectly confirms that the proportion of quartz in the flotation concentrate decreases), thereby improving the grade of magnesium-containing minerals (the MgO content is increased to more than 43%).

[0023] (3) The magnesium-containing mineral obtained by the present invention can be applied to the fields of silica-magnesium gel extraction, magnesium oxide chemical leaching, etc., and the magnetite can be applied to the fields of aerated bricks, cement, microcrystalline glass, etc. for building materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figure is a simplified diagram of the process for enriching magnesium-containing minerals in asbestos tailings;

[0025] Figure 2 This is the XRD pattern of asbestos tailings. DETAILED DESCRIPTION

[0026] Combination Figure 1 , the present invention is further described:

[0027] A method for enriching magnesium-containing minerals in asbestos tailings, the specific implementation steps are as follows:

[0028] Example 1

[0029] The main mineral phases of an asbestos tailing include serpentine (L), chrysotile (Ch), quartz (Q), magnetite (Ma), a small amount of albite (A), plagioclase (Mi), calcite (C), etc. Its XRD spectrum is shown in Figure 2 , the specific ingredients are shown in Table 1 below;

[0030] (1) A jaw crusher was used to crush asbestos tailings (particle size composition was +8mm, 1.6%; 3~8mm, 90.3%; -3mm, 8.1%) to less than 3mm. The asbestos tailings below 3mm were ground using a Φ200×240 rod mill. The grinding medium was a steel rod weighing 13.2kg. The grinding medium weight ratio was Φ20mm:Φ16mm:Φ14mm=6.32kg:4.36kg:2.02kg. The feed rate was 1.0kg / time. The grinding mass concentration was 50%. The grinding time was 6min. The particle size composition of the asbestos tailings after grinding was +0.45mm content 1.5%, 0.105~0.45mm content 80.6%, -0.105mm content 17.9%.

[0031] (2) The asbestos tailings after grinding are screened by wet screening to remove the +0.45mm particle size, which is mainly short-flocculated chrysotile; the -0.45mm asbestos tailings are screened by a Φ125mm hydraulic classifier to remove the -0.105mm particle size, and the water flow of the hydraulic classifier is controlled at 140L / h; the overflow of the classifier is fine-grained asbestos tailings; the classified sand is coarse-grained asbestos tailings, and the coarse-grained asbestos tailings have a particle size composition of 0.105~0.45mm and a content of 95.5%;

[0032] (3) The graded sediment (coarse-grained asbestos tailings) is separated into quartz and feldspar by mixed flotation. The flotation is carried out using a composite modified carboxyl starch as an inhibitor (dosage 500 g / t) and an amphoteric collector ND-3 (neutral flotation agent mentioned in patent publication number CN108176518A) as a collector and frother (dosage 810 g / t). The inhibitor is first added to mix the slurry for 1 min, and then the collector is added to mix the slurry for 2 min. The slurry is aerated for 30 s and the scraping time is 3 min. The floating foam is the mixed flotation tailings of quartz and feldspar. The sediment in the trough is the flotation concentrate, i.e., the enriched magnesium-containing minerals and magnetite.

[0033] (4) The flotation concentrate and the fine-grained asbestos tailings obtained by classification are ground in a ball mill. The grinding medium is a steel ball weighing 8.5 kg. The weight ratio of the grinding medium is Φ20 mm: Φ14 mm: Φ10 mm = 2.60 kg: 4.25 kg: 1.65 kg. The feed rate is 1.0 kg / time. The grinding mass concentration is 50%. The grinding time is 15 min. The particle size composition of the product after grinding is +0.074 mm content 5.9%; 0.038~0.074 mm content 81.4%, -0.038 mm content 12.7%;

[0034] (5) The mixture of the flotation concentrate after grinding and the fine-grained asbestos tailings obtained by classification is magnetically separated by a drum magnetic separator with a magnetic field intensity of 1500 Gs. The product adhering to the magnetic drum is the magnetic tailings (i.e., magnetite); the remaining minerals are the magnetic concentrate, i.e., magnesium-containing minerals whose main component is serpentine.

[0035] The chemical composition of different products was analyzed by X-ray fluorescence spectrometer (XRF), see Table 1:

[0036]

[0037] Calculated based on asbestos tailings as 100.00%, the content of short flocculent chrysotile obtained by pre-enrichment is 1.2%, the yield of flotation concentrate is 84.72%, and the yield of flotation concentrate combined with fine-grained asbestos tailings and primary magnetic separation of magnesium-containing minerals is 71.08%.

[0038] Comparative Example 1

[0039] When the asbestos tailings are not enriched by the method of the present invention, the index is still the original asbestos tailings index:

[0040]

[0041] The above embodiments are only descriptions of preferred examples of the present invention and do not limit the scope of the present invention. Without departing from the principle of the present invention, all forms of changes should fall within the scope of protection of the claims of the present invention.

Claims

1. A method for enriching magnesium-containing minerals in asbestos tailings, characterized in that The steps include: (1) Directly crush or grind the asbestos tailings to control the dissociation particle size of the mineral to -0.71 mm, and at the same time control the particle size to be no less than the lower limit of flotation; (2) Controlling the grading cutting particle size to be 0.105 mm to 0.038 mm, and grading the crushed or ground asbestos tailings to obtain fine-grained asbestos tailings and coarse-grained asbestos tailings; flotating the coarse-grained asbestos tailings by a quartz and feldspar mixed flotation method, wherein the inhibitor is modified carboxyl starch, the collector and frother is an amphoteric collector or a cationic collector, the flotation foam is the flotation tailings, and the sediment is the flotation concentrate; the grading is hydraulic grading, airflow grading or dry and wet screening; the flotation concentrate is subjected to one or more scavenging; (3) Grinding the fine-grained asbestos tailings and flotation concentrate obtained by classification in step (2) together to obtain a mineral with a particle size of -0.105 mm; then magnetically separating the mineral, controlling the magnetic field strength to be no greater than 4000 Gs, to obtain magnetite and magnesium-containing minerals; and re-grinding and re-magnetically separating the magnetite and magnesium-containing minerals after magnetic separation.

2. The method for enriching magnesium-containing minerals in asbestos tailings according to claim 1, characterized in that: The fine-grained asbestos tailings and flotation concentrate obtained by classification in step (2) are directly subjected to magnetic separation without grinding.

3. A method for enriching magnesium-containing minerals in asbestos tailings according to claim 1 or 2, characterized in that: The main components of the magnetite after magnetic separation in step (3) are monomer magnetite or a combination or inclusion of magnetite and serpentine magnesium-containing minerals; the main component of the magnesium-containing minerals is serpentine.

4. The method for enriching magnesium-containing minerals in asbestos tailings according to claim 1, characterized in that: The amount of flotation depressant used in step (2) is ≤1.0 kg / t.

5. The method for enriching magnesium-containing minerals in asbestos tailings according to claim 1, characterized in that: The amount of the flotation collector and frother used in step (2) is ≤1.5kg / t.