Method for forming semiconductor structure
By forming and removing work function material layers on different regions of the semiconductor structure and accurately controlling the thickness using the atomic layer etching process, the problem of difficulty in forming different threshold voltage transistors in the prior art is solved, and device performance and production efficiency are improved.
Patent Information
- Application Number
- CN202010018878.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-01-08
AI Technical Summary
It is difficult for the prior art to form transistors with different threshold voltages on the same substrate, and the existing processes are complex and easily lead to unstable device performance and threshold voltage drift.
By forming the same type of work function material layer on different regions of the semiconductor structure and directionally remove using the atomic layer etching process, the material thickness is accurately controlled, lateral etching is avoided, and the process flow is simplified.
The device with different threshold voltages is formed on the same substrate, which improves the uniformity of device performance and production efficiency, and avoids threshold voltage drift.
Smart Images

Figure CN113097136B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Art
[0002] In the field of integrated circuit manufacturing, as the size of transistors continues to shrink, the physical limits of devices have an increasingly greater impact on device preparation, and it becomes more difficult to scale down the characteristic dimensions of devices. The difficulty in the field of transistor and circuit manufacturing has also increased significantly.
[0003] In order to meet the requirements, transistors with different functions need to be formed on the same substrate. In the prior art, a work function layer is used to adjust the performance of transistors formed by a post-metal gate process to meet the requirements of transistors with different functions.
[0004] However, the performance of existing transistors still needs to be improved. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for forming a semiconductor structure to improve the performance of transistors.
[0006] To solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, the substrate comprising a first region, a second region and a third region; forming a first work function material layer on the first region, the second region and the third region of the substrate; forming a second work function material layer on the first work function material layer, the second work function material layer and the first work function material layer having the same work function type; removing the first work function material layer and the second work function material layer on the first region; removing the second work function material layer on the second region.
[0007] Optionally, the method for removing the second work function material layer on the second region includes: forming a first mask layer on the surface of the substrate, the first mask layer exposing the top surface of the second work function material layer on the second region; etching the second work function material layer using the first mask layer as a mask to form a second work function structure in the second region.
[0008] Optionally, the method for removing the first work function material layer and the second work function material layer on the first region includes: forming a second mask layer on the surface of the substrate, the second mask layer exposing the top surface of the second work function material layer on the first region; etching the second work function material layer and the first work function material layer using the second mask layer as a mask until the substrate surface is exposed.
[0009] Optionally, the process of removing the first work function material layer and the second work function material layer includes a first atomic layer etching process; the first atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a first modification treatment on the surface to be etched to form a first modified layer; and removing the first modified layer.
[0010] Optionally, the modification process of the first work function material layer and the second work function material layer includes an oxidation process.
[0011] Optionally, the material of the first work function material layer and the second work function material layer is a P-type work function material; or, the material of the first work function material layer and the second work function material layer is an N-type work function material; the P-type work function material includes titanium nitride or tantalum nitride; the N-type work function material includes titanium aluminum.
[0012] Optionally, the substrate also includes a fourth region; the first work function material layer is also located on the fourth region; the second work function material layer is also located on the fourth region; after forming the second work function material layer, it also includes: forming a third work function material layer on the second work function material layer; before removing the first work function material layer and the second work function material layer on the first region, removing the third work function material layer on the first region; before removing the second work function material layer on the second region, removing the third work function material layer on the second region; removing the third work function material layer on the third region.
[0013] Optionally, the material of the third work function material layer has the same work function type as that of the second work function material layer.
[0014] Optionally, before forming the first work function material layer on the substrate, it also includes: forming a dielectric layer on the substrate; forming a first gate opening located on the first area in the dielectric layer; forming a second gate opening located on the second area in the dielectric layer, and forming a third gate opening located on the third area in the dielectric layer.
[0015] Optionally, before forming the first work function material layer, it also includes: forming a gate dielectric layer on the inner wall of the first gate opening, the inner wall of the second gate opening and the inner wall of the third gate opening; forming a protective layer on the gate dielectric layer, and the first work function material layer is located on the protective layer.
[0016] Optionally, after forming the protection layer, the method further includes: forming a stop layer on the protection layer, wherein the first work function material layer is located on the stop layer.
[0017] Optionally, after removing the second work function material layer on the second region, the method further includes: forming a fourth work function material layer on the first region, the second region and the third region, wherein the material of the fourth work function material layer has a work function type opposite to that of the second work function material layer.
[0018] Optionally, after forming the fourth work function material layer, the method further includes: removing the fourth work function material layer on either one or both of the third and fourth regions.
[0019] Optionally, the process of removing the fourth work function material layer includes a second atomic layer etching process; the second atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a second modification treatment on the surface to be etched to form a second modified layer; and removing the second modified layer.
[0020] Optionally, the modification process for the fourth work function material layer includes an oxidation process.
[0021] Optionally, after forming the second work function structure and the third work function structure, the method further includes: forming a gate layer on the first region, the second region and the third region.
[0022] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0023] In the method of the technical solution of the present invention, by first forming the first work function material layer and the second work function material layer on the first area, the second area and the third area, and then removing the first work function material layer and the second work function material layer on the first area, and removing the second work function material layer on the second area, the work function structures formed on the first area, the second area and the third area have different thicknesses, thereby meeting the need to form devices with different threshold voltages on the same substrate. The first work function material layer and the second work function material layer are first formed, and then removed separately according to the needs of the first area, the second area and the third area, thereby simplifying the process and improving production efficiency.
[0024] Furthermore, the process of removing the first work function material layer and the second work function material layer includes a first atomic layer etching process, wherein the first atomic layer etching process first modifies the surface to be etched to form a modified layer, and then removes the modified layer, so that the first atomic layer etching process can directionally remove the first work function material layer and the second work function material layer to be removed, thereby avoiding the lateral etching that occurs when the first work function material layer and the second work function material layer are removed by a wet etching process when they are not modified, and the lateral etching causes the device threshold voltage of the second zone and the device threshold voltage of the third zone to drift; at the same time, the first atomic layer etching process can accurately control the thickness of the first work function material layer and the second work function material layer to be removed, so that the thickness of the work function structure on the second zone and the work function structure on the third zone formed can be accurately controlled, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved.
[0025] Furthermore, the process of removing the fourth work function material layer includes a second atomic layer etching process, wherein the second atomic layer etching process first modifies the surface to be etched to form a modified layer, and then removes the modified layer, so that the second atomic layer etching process can directionally remove the fourth work function material layer to be removed, avoiding lateral etching when the fourth work function material layer is removed by a wet etching process when it is not modified, and the lateral etching causes the threshold voltage of the device formed on the first area and the device formed on the second area to drift; at the same time, the second atomic layer etching process can accurately control the thickness of the fourth work function material layer to be removed, so that the thickness of the work function structure formed on the first area and the work function structure formed on the second area can be accurately controlled, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic cross-sectional structural diagram of a semiconductor structure in one embodiment;
[0027] Figures 2 to 11 It is a schematic cross-sectional structure diagram of a semiconductor structure forming process in an embodiment of the present invention. DETAILED DESCRIPTION
[0028] As described in the background art, the performance of existing transistors still needs to be improved. Now, an analysis and description will be given in conjunction with specific embodiments.
[0029] Figure 1 It is a schematic cross-sectional structure diagram of a semiconductor structure in one embodiment.
[0030] Please refer to Figure 1, comprising: a substrate 100, the substrate comprising a first region I, a second region II, a third region III and a fourth region IV; a dielectric layer 101 located on the substrate 100; a first gate opening (not shown) located in the dielectric layer 101 on the first region I, a second gate opening (not shown) located in the dielectric layer 101 on the second region II, a third gate opening (not shown) located in the dielectric layer 101 on the third region III, a fourth gate opening (not shown) located in the dielectric layer 101 on the fourth region IV, the first gate opening sidewall, the second gate opening sidewall, the third gate opening sidewall and the fourth gate opening sidewall having a spacer structure 102; a gate dielectric layer 103 located in the first gate opening, the second gate opening, the third gate opening and the fourth gate opening, a protective layer 104 located on the gate dielectric layer 103, and a stop layer 105 located on the protective layer 104; a stop layer 105 located in the first region I a first work function structure on the stop layer 105 in the second region II, the first work function structure including a fourth work function layer 109; a second work function structure on the stop layer 105 in the second region II, the second work function structure including a third work function layer 108 and a fourth work function layer 109 on the third work function layer 108; a third work function structure on the stop layer 105 in the third region III, the third work function structure including a second work function layer 107, a third work function layer 108 on the second work function layer 107, and a fourth work function layer 109 on the third work function layer 108; a fourth work function structure on the stop layer 105 in the fourth region IV, the fourth work function structure including a first work function layer 106, a second work function layer 107 on the first work function layer 106, a third work function layer 108 on the second work function layer 107, and a fourth work function layer 109 on the third work function layer 108.
[0031] The first region I, the second region II, the third region III and the fourth region IV of the semiconductor structure need to form devices with different threshold voltages to meet the requirements of diversified device performance, so that the work function structures formed on the first region I, the second region II, the third region III and the fourth region IV have different thicknesses. The steps of forming the first work function structure, the second work function structure, the third work function structure and the fourth work function structure are: forming a first work function material layer in the first region I, the second region II, the third region III and the fourth region IV; forming a first mask layer to remove the first work function material layer on the third region III; forming a second work function material layer in the first region I, the second region II, the third region III and the fourth region IV; forming a second mask layer to remove the second work function material layer and the first work function material layer on the second region II; forming a third work function material layer in the first region I, the second region II, the third region III and the fourth region IV; forming a third mask layer to remove the third work function material layer, the second work function material layer and the first work function material layer on the first region I; forming a fourth work function material layer in the first region I, the second region II, the third region III and the fourth region IV.
[0032] The materials of the first work function layer, the second work function layer and the third work function layer are the same, and the material of the fourth work function layer is different from the materials of the first work function layer, the second work function layer and the third work function layer. In the process of forming the first work function structure, the second work function structure, the third work function structure and the fourth work function structure, it is necessary to form the first work function material layer, the second work function material layer and the third work function material layer three times, and then remove the first work function material layer, the second work function material layer and the third work function material layer three times, and the process flow is relatively complicated. At the same time, the process of removing the first work function material layer, the second work function material layer and the third work function material layer mostly adopts an isotropic wet etching process. When removing the work function material layer, the isotropic wet etching process is easy to etch laterally, thereby affecting the work function structure in other areas, so that the threshold voltage of the formed work function structure drifts, making the performance of the semiconductor structure unstable.
[0033] In order to solve the above problems, the technical problem of the present invention provides a method for forming a semiconductor structure, by first forming a first work function material layer and a second work function material layer on the first region, the second region and the third region, and then removing the first work function material layer and the second work function material layer on the first region, and removing the second work function material layer on the second region, respectively, so that the work function structures formed on the first region, the second region and the third region have different thicknesses, thereby meeting the need to form devices with different threshold voltages on the same substrate. The materials of the first work function material layer and the second work function material layer are the same, so that the first work function material layer and the second work function material layer only need to be formed by one formation process, thereby simplifying the process and improving production efficiency.
[0034] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0035] Figures 2 to 11 It is a schematic cross-sectional structure diagram of the semiconductor structure forming process in an embodiment of the present invention.
[0036] Please refer to Figure 2 , providing a substrate 200, wherein the substrate 200 includes a first region I, a second region II and a third region III.
[0037] In this embodiment, the substrate 200 further includes a fourth region IV. In other embodiments, the fourth region IV may not be included.
[0038] The first region I, the second region II, the third region III and the fourth region IV are subsequently used to form devices with different threshold voltages.
[0039] In this embodiment, the material of the substrate 200 is single crystal silicon; in other embodiments, the substrate may also be a semiconductor material such as polycrystalline silicon, germanium, silicon germanium, gallium arsenide or silicon on insulator.
[0040] Please refer to Figure 3 , a dielectric layer 201 is formed on the substrate 200; a first gate opening 301 is formed in the dielectric layer 201 and located on the first region I; a second gate opening 302 is formed in the dielectric layer 201 and located on the second region II; a third gate opening 303 is formed in the dielectric layer 201 and located on the third region III; and a fourth gate opening 304 is formed in the dielectric layer 201 and located on the fourth region IV.
[0041] The method for forming the first gate opening 301, the second gate opening 302, the third gate opening 303 and the fourth gate opening 304 comprises: forming a dummy gate structure (not shown) on the first region I, the second region II, the third region III and the fourth region IV; forming a sidewall 202 on the sidewall of the dummy gate structure; forming a dielectric layer 201 on the substrate 200, wherein the dielectric layer 201 exposes the top surface of the dummy gate structure; removing the dummy gate structure, forming a first gate opening 301 in the first region I, forming a second gate opening 302 in the second region II, forming a third gate opening 303 in the third region III, and forming a fourth gate opening 304 in the fourth region IV.
[0042] The dummy gate structure includes a dummy gate dielectric layer (not shown) and a dummy gate layer (not shown) located on the dummy gate dielectric layer.
[0043] In this embodiment, the material of the dummy gate dielectric layer includes silicon oxide; and the material of the dummy gate layer includes polysilicon.
[0044] The method for forming the dielectric layer 201 includes: forming a dielectric material layer (not shown) on the top surface of the dummy gate structure and the sidewall surface of the spacer 202; and planarizing the dielectric material layer until the top surface of the dummy gate structure is exposed to form the dielectric layer 201.
[0045] The material of the dielectric layer 201 includes silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride or silicon carbonitride. The process of forming the dielectric material layer includes chemical vapor deposition process or atomic layer deposition process.
[0046] In this embodiment, the material of the dielectric layer 201 includes silicon oxide; the process of forming the dielectric material layer includes a chemical vapor deposition process, and the chemical vapor deposition process can quickly form a dielectric material layer with a relatively thick thickness and a dense structure.
[0047] Please refer to Figure 4 A gate dielectric layer 203 is formed on the inner wall of the first gate opening 301 , the inner wall of the second gate opening 302 , the inner wall of the third gate opening 303 and the inner wall of the fourth gate opening 304 ; and a protection layer 204 is formed on the gate dielectric layer 203 .
[0048] The protection layer 204 can protect the gate dielectric layer 203 to prevent the gate dielectric layer 203 from being damaged in subsequent processes.
[0049] The material of the gate dielectric layer 203 is a high-K (relative dielectric constant greater than 3.9) material, and the high-K material includes hafnium oxide or aluminum oxide; the material of the protective layer 204 includes titanium nitride or tantalum nitride; the process for forming the gate dielectric layer 203 includes an atomic layer deposition process or a chemical vapor deposition process; the process for forming the protective layer 204 includes an atomic layer deposition process or a chemical vapor deposition process.
[0050] In this embodiment, the material of the gate dielectric layer 203 includes hafnium oxide; the material of the protective layer 204 includes titanium nitride; the process for forming the gate dielectric layer 203 includes an atomic layer deposition process, and the atomic layer deposition process can form a gate dielectric layer 203 with a dense structure and a thin thickness; the process for forming the protective layer 204 includes an atomic layer deposition process, and the atomic layer deposition process can form a protective layer 204 with a dense structure and a thin thickness.
[0051] Please continue to refer to Figure 4 , a stop layer 205 is formed on the protection layer 204 .
[0052] The material of the stop layer 205 includes tantalum nitride or titanium nitride; the process of forming the stop layer 205 includes an atomic layer deposition process or a chemical vapor deposition process.
[0053] In this embodiment, the material of the stop layer 205 includes tantalum nitride; the process of forming the stop layer 205 includes an atomic layer deposition process, and the atomic layer deposition process can form a stop layer 205 with a dense structure and a relatively thin thickness.
[0054] The stop layer 205 serves as an etching stop layer for subsequently removing the first work function material layer and the second work function material layer, thereby preventing the protection layer 204 and the gate dielectric layer 203 from being damaged by over-etching.
[0055] In other embodiments, the stop layer may not be formed.
[0056] Please refer to Figure 5 , a first work function material layer 206 is formed on the first region I, the second region II and the third region III of the substrate 200 ; and a second work function material layer 207 is formed on the first work function material layer 206 .
[0057] In this embodiment, the process further includes forming a first work function material layer 206 on the fourth region IV; and forming a second work function material layer 207 on the first work function material layer 206 .
[0058] In other embodiments, the fourth region IV may not be formed.
[0059] The work function type of the second work function material layer 207 is the same as that of the first work function material layer 206. Specifically, the materials of the first work function material layer 206 and the second work function material layer 207 are P-type work function materials; or, the materials of the first work function material layer 206 and the second work function material layer 207 are N-type work function materials; the P-type work function material includes titanium nitride or tantalum nitride; the N-type work function material includes titanium aluminum.
[0060] In this embodiment, the material of the second work function material layer 207 includes a P-type work function material, and the P-type work function material includes titanium nitride; the material of the first work function material layer 206 includes a P-type work function material, and the P-type work function material includes titanium nitride.
[0061] The process of forming the first work function material layer 206 includes an atomic layer deposition process or a chemical vapor deposition process; the process of forming the second work function material layer 207 includes an atomic layer deposition process or a chemical vapor deposition process.
[0062] In this embodiment, the process for forming the first work function material layer 206 includes an atomic layer deposition process, which can form a first work function material layer 206 with a dense structure and a thin thickness; the process for forming the second work function material layer 207 includes an atomic layer deposition process, which can form a second work function material layer 207 with a dense structure and a thin thickness.
[0063] In this embodiment, the material of the first work function material layer 206 is the same as the material of the second work function material layer 207 , and the first work function material layer 206 and the second work function material layer 207 can be formed by one process, thereby saving process flow and improving production efficiency.
[0064] In other embodiments, the material of the second work function material layer and the material of the first work function material layer may be P-type work function materials of different materials, and the P-type work function material includes titanium nitride or tantalum nitride.
[0065] In another embodiment, the material of the second work function material layer and the material of the first work function material layer may be the same N-type work function material, and the N-type work function material includes titanium aluminum.
[0066] In another embodiment, the material of the second work function material layer and the material of the first work function material layer may be N-type work function materials of different materials, and the N-type work function material includes titanium aluminum.
[0067] Please continue to refer to Figure 5 , a third work function material layer 208 is formed on the second work function material layer 207 .
[0068] The material of the third work function material layer 208 has the same work function type as that of the second work function material layer 207 , and the material of the third work function material layer 208 has the same work function type as that of the first work function material layer 206 .
[0069] Specifically, the materials of the third work function material layer 208 and the second work function material layer 207 are P-type work function materials; or, the materials of the third work function material layer 208 and the second work function material layer 207 are N-type work function materials; the P-type work function material includes titanium nitride or tantalum nitride; the N-type work function material includes titanium aluminum.
[0070] In the present embodiment, the material of the third work function material layer 208 includes a P-type work function material, and the P-type work function material includes titanium nitride.
[0071] The process of forming the third work function material layer 208 includes an atomic layer deposition process or a chemical vapor deposition process. In this embodiment, the process of forming the third work function material layer 208 includes an atomic layer deposition process, which can form a third work function material layer 208 with a dense structure and a relatively thin thickness.
[0072] In this embodiment, the materials of the first work function material layer 206, the second work function material layer 207 and the third work function material layer 208 are the same, which is titanium nitride. Therefore, the first work function material layer 206, the second work function material layer 207 and the third work function material layer 208 can be formed by an atomic layer deposition process, thereby simplifying the process flow and improving production efficiency.
[0073] In this embodiment, a third work function material layer 208 is further formed on the second work function material layer 207 in the fourth region IV.
[0074] In other embodiments, the fourth region IV is not formed, so that the third work function material layer may not be formed in the first region I, the second region II, and the third region III.
[0075] In other embodiments, the material of the third work function material layer and the material of the second work function material layer may be P-type work function materials of different materials, and the P-type work function material includes titanium nitride or tantalum nitride.
[0076] In another embodiment, the material of the third work function material layer and the material of the second work function material layer may be the same N-type work function material, and the N-type work function material includes titanium aluminum.
[0077] In another embodiment, the material of the third work function material layer and the material of the second work function material layer may be N-type work function materials of different materials, and the N-type work function material includes titanium aluminum.
[0078] Please refer to Figure 6 , remove the third work function material layer 208 on the third region III.
[0079] The method for removing the third work function material layer 208 on the third region III includes: forming a third mask layer (not shown) on the substrate 200, wherein the third mask layer exposes the third work function material layer 208 on the surface of the third region III; and etching the third work function material layer 208 using the third mask layer as a mask until the surface of the second work function material layer 207 is exposed.
[0080] The process of removing the third work function material layer 208 includes a first atomic layer etching process; the first atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a first modification treatment on the surface to be etched to form a first modified layer (not shown); and removing the first modified layer.
[0081] The modification process for the third work function material layer 208 includes an oxidation process.
[0082] In this embodiment, the third work function material layer 208 is modified by an ozone oxidation process; the material of the first modified layer includes titanium dioxide; and the process of removing the first modified layer includes a wet etching process.
[0083] The material of the third work function material layer 208 includes titanium nitride. The titanium nitride reacts with the ozone to generate titanium dioxide and nitrogen-containing gas. The nitrogen-containing gas is drawn out of the cavity along with other gases, so that the titanium nitride is modified to form titanium dioxide.
[0084] A wet etching process is used to remove the first modified layer, wherein the etching solution of the wet etching process includes a hydrogen fluoride solution, and the hydrogen fluoride solution has a large etching selectivity for titanium dioxide, so that while removing the first modified layer, less damage is caused to the unmodified titanium nitride, thereby being able to accurately control the thickness of the third work function material layer 208 to be removed.
[0085] In other embodiments, the third work function material layer is modified by oxygen-containing plasma treatment.
[0086] The third work function material layer 208 is removed by a first atomic layer etching process. The first atomic layer etching process first modifies the surface to be etched to form a first modified layer, and then removes the first modified layer, so that the first atomic layer etching process can directionally remove the third work function material layer 208 to be removed. The lateral etching that occurs when the third work function material layer 208 is removed by a wet etching process without modification is avoided, and the lateral etching causes the device threshold voltage of the first zone, the device threshold voltage of the second zone, and the device threshold voltage of the fourth zone to drift; at the same time, the first atomic layer etching process can accurately control the thickness of the third work function material layer 208 to be removed, so that the thickness of the work function structure on the third zone formed is accurately controllable, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved.
[0087] Please refer to Figure 7 , remove the third work function material layer 208 and the second work function material layer 207 on the second region II.
[0088] The method for removing the third work function material layer 208 and the second work function material layer 207 on the second region II includes: forming a second mask layer (not shown) on the substrate 200, the second mask layer exposing the third work function material layer 208 on the surface of the second region II; etching the third work function material layer 208 and the second work function material layer 207 using the second mask layer as a mask until the surface of the first work function material layer 206 is exposed.
[0089] The process of removing the third work function material layer 208 and the second work function material layer 207 includes a first atomic layer etching process; the first atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a first modification treatment on the surface to be etched to form a first modified layer (not shown); and removing the first modified layer.
[0090] The modification process of the third work function material layer 208 and the second work function material layer 207 includes an oxidation process.
[0091] In this embodiment, the third work function material layer 208 and the second work function material layer 207 are modified by an ozone oxidation process; the material of the first modified layer includes titanium dioxide; and the process of removing the first modified layer includes a wet etching process.
[0092] The materials of the third work function material layer 208 and the second work function material layer 207 include titanium nitride. The titanium nitride reacts with the ozone to generate titanium dioxide and nitrogen-containing gas. The nitrogen-containing gas is drawn out of the cavity along with other gases, so that the titanium nitride is modified to form titanium dioxide.
[0093] A wet etching process is used to remove the first modified layer, wherein the etching solution of the wet etching process includes a hydrogen fluoride solution, and the hydrogen fluoride solution has a large etching selectivity for titanium dioxide, so that while removing the first modified layer, less damage is caused to the unmodified titanium nitride, thereby being able to accurately control the thickness of the third work function material layer 208 and the second work function material layer 207.
[0094] In other embodiments, the modification treatment of the third work function material layer and the second work function material layer is performed by plasma treatment containing oxygen.
[0095] The third work function material layer 208 and the second work function material layer 207 are removed by a first atomic layer etching process. The first atomic layer etching process first modifies the surface to be etched to form a first modified layer, and then removes the first modified layer, so that the first atomic layer etching process can directionally remove the third work function material layer 208 and the second work function material layer 207 to be removed. The lateral etching that occurs when the third work function material layer 208 and the second work function material layer 207 are removed by a wet etching process without modification is avoided, and the lateral etching causes the device threshold voltage of the first area, the device threshold voltage of the third area, and the device threshold voltage of the fourth area to drift; at the same time, the first atomic layer etching process can accurately control the thickness of the third work function material layer 208 and the second work function material layer 207 to be removed, so that the thickness of the work function structure on the second area formed is accurately controllable, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved.
[0096] Please refer to Figure 8 , the third work function material layer 208 , the second work function material layer 207 and the first work function material layer 206 on the first region I are removed.
[0097] The method for removing the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 on the first region I includes: forming a first mask layer (not shown) on the substrate 200, the first mask layer exposing the third work function material layer 208 on the surface of the first region I; etching the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 using the first mask layer as a mask until the surface of the stop layer 205 is exposed.
[0098] The process of removing the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 includes a first atomic layer etching process; the first atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a first modification treatment on the surface to be etched to form a first modified layer (not shown); and removing the first modified layer.
[0099] The modification process for the third work function material layer 208 , the second work function material layer 207 and the first work function material layer 206 includes an oxidation process.
[0100] In this embodiment, the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 are modified by an ozone oxidation process; the material of the first modified layer includes titanium dioxide; and the process for removing the first modified layer includes a wet etching process.
[0101] The materials of the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 include titanium nitride, which reacts with the ozone to generate titanium dioxide and nitrogen-containing gas. The nitrogen-containing gas is drawn out of the cavity along with other gases, so that the titanium nitride is modified to form titanium dioxide.
[0102] A wet etching process is used to remove the first modified layer, wherein the etching solution of the wet etching process includes a hydrogen fluoride solution, and the hydrogen fluoride solution has a large etching selectivity for titanium dioxide, so that while removing the first modified layer, less damage is caused to the unmodified titanium nitride, thereby being able to accurately control the thickness of the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206.
[0103] In other embodiments, the modification treatment of the third work function material layer, the second work function material layer and the first work function material layer is performed by plasma treatment containing oxygen.
[0104] The first atomic layer etching process is used to remove the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206. The first atomic layer etching process first modifies the surface to be etched to form a first modified layer, and then removes the first modified layer, so that the first atomic layer etching process can directionally remove the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 that need to be removed. The lateral etching that occurs when the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 are removed by a wet etching process without modification is avoided, and the lateral etching causes the device threshold voltage of the second zone, the device threshold voltage of the third zone and the device threshold voltage of the fourth zone to drift; at the same time, the first atomic layer etching process can accurately control the thickness of the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 to be removed, so that the thickness of the work function structure on the first zone formed is accurately controllable, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved.
[0105] Please refer to Fig. 9 , a fourth work function material layer 209 is formed on the first region I, the second region II and the third region III.
[0106] In this embodiment, a fourth work function material layer 209 is further formed on the fourth region IV.
[0107] In other embodiments, the fourth region IV is not formed.
[0108] The material of the fourth work function material layer 209 has a work function type opposite to that of the second work function material layer 207. Specifically, if the material of the second work function material layer 207 is a P-type work function material, then the material of the fourth work function material layer 209 is an N-type work function material; or, if the material of the second work function material layer 207 is an N-type work function material, then the material of the fourth work function material layer 209 is a P-type work function material; the P-type work function material includes titanium nitride or tantalum nitride; and the N-type work function material includes titanium aluminum.
[0109] In this embodiment, the material of the fourth work function material layer 209 is an N-type work function material, and the N-type work function material includes titanium aluminum.
[0110] The process of forming the fourth work function material layer 209 includes an atomic layer deposition process or a chemical vapor deposition process. In this embodiment, the process of forming the fourth work function material layer 209 includes an atomic layer deposition process, which can form a fourth work function material layer 209 with a dense structure and a relatively thin thickness.
[0111] The work function type of the fourth work function material layer 209 is opposite to that of the second work function material layer 207, and the work function type of the fourth work function material layer 209 is also opposite to that of the third work function material layer 208 and the first work function material layer 206. The fourth work function material layer 209 is used to adjust the threshold voltages of the formed first work function material layer 206, the second work function material layer 207 and the third work function material layer 208, so that the threshold voltages of the devices in the first area, the threshold voltages of the devices in the second area and the threshold voltages of the devices in the third area meet different requirements.
[0112] In other embodiments, the work function type of the second work function material layer is N-type, and the material of the fourth work function material layer is P-type work function material, and the P-type work function material includes titanium nitride or tantalum nitride.
[0113] Please refer to Fig.10 , remove the fourth work function material layer 209 on either or both of the third region III and the fourth region IV.
[0114] In this embodiment, the fourth work function material layer 209 on the third region III is removed.
[0115] The process of removing the fourth work function material layer 209 includes a second atomic layer etching process; the second atomic layer etching process includes a single or multiple cycle process; each cycle process includes: performing a second modification treatment on the surface to be etched to form a second modified layer; and removing the second modified layer.
[0116] The fourth work function material layer 209 is modified by an oxidation process. In this embodiment, the fourth work function material layer 209 is modified by ozone oxidation; the material of the second modified layer includes titanium oxide and aluminum oxide; and the process for removing the second modified layer includes a wet etching process.
[0117] A wet etching process is used to remove the second modified layer, wherein the etching solution of the wet etching process includes a hydrogen fluoride solution, and the hydrogen fluoride solution has a large etching selectivity for titanium oxide and aluminum oxide, so that while the second modified layer can be removed, less damage is caused to the unmodified titanium aluminum, thereby accurately controlling the thickness of the fourth work function material layer 209 to be removed.
[0118] The fourth work function material layer 209 is removed by a second atomic layer etching process. The second atomic layer etching process first modifies the surface to be etched to form a modified layer, and then removes the modified layer, so that the second atomic layer etching process can directionally remove the fourth work function material layer 209 to be removed, avoiding lateral etching when the fourth work function material layer 209 is removed by a wet etching process without modification, and the lateral etching causes the device threshold voltage on the first area, the device threshold voltage on the second area, and the device threshold voltage on the fourth area to drift; at the same time, the second atomic layer etching process can accurately control the thickness of the fourth work function material layer 209 to be removed, so that the thickness of the work function structure on the third area formed is accurately controllable, so that the performance uniformity of the formed device is better. In summary, the performance of the semiconductor structure is improved.
[0119] In other embodiments, the fourth work function material layer on the fourth region IV is removed, or the fourth work function material layer on the third region III and the fourth region IV is removed.
[0120] Please refer to Fig.11 , a gate layer 210 is formed on the first region I, the second region II and the third region III.
[0121] In this embodiment, a gate layer 210 is further formed on the fourth region IV.
[0122] In other embodiments, the fourth region IV is not formed.
[0123] The method for forming the gate layer 210 includes: forming a gate material layer (not shown) on the first region I, the second region II, the third region III and the fourth region IV; planarizing the gate material layer, the fourth work function material layer 209, the third work function material layer 208, the second work function material layer 207 and the first work function material layer 206 until the surface of the dielectric layer 201 is exposed to form the gate layer 210.
[0124] The material of the gate layer 210 includes metal, and the metal includes tungsten.
[0125] Thus, in the semiconductor structure formed, the devices in the first region I, the second region II, the third region III and the fourth region IV have different threshold voltages. The method for forming the semiconductor structure is simplified, and the production efficiency is improved.
[0126] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, It is characterized in that include: providing a substrate, the substrate comprising a first region, a second region, a third region, and a fourth region; forming a first work function material layer on the first region, the second region, the third region and the fourth region of the substrate; forming a second work function material layer on the first work function material layer, wherein the second work function material layer has the same work function type as the first work function material layer; forming a third work function material layer on the second work function material layer, wherein the material of the third work function material layer has the same work function type as that of the second work function material layer; removing the first work function material layer, the second work function material layer and the third work function material layer on the first region; removing the second work function material layer and the third work function material layer on the second region; removing the third work function material layer on the third region; After removing the first work function material layer, the second work function material layer and the third work function material layer, a fourth work function material layer is formed on the first area, the second area and the third area, and the material of the fourth work function material layer has a work function type opposite to that of the second work function material layer.
2. The method for forming a semiconductor structure according to claim 1, It is characterized in that The method for removing the second work function material layer on the second region includes: forming a first mask layer on the surface of the substrate, wherein the first mask layer exposes the top surface of the second work function material layer on the second region; etching the second work function material layer using the first mask layer as a mask to form a second work function structure in the second region.
3. The method for forming a semiconductor structure according to claim 1, It is characterized in that The method for removing the first work function material layer and the second work function material layer on the first region includes: forming a second mask layer on the surface of the substrate, the second mask layer exposing the top surface of the second work function material layer on the first region; etching the second work function material layer and the first work function material layer using the second mask layer as a mask until the substrate surface is exposed.
4. The method for forming a semiconductor structure according to claim 1, It is characterized in that The process of removing the first work function material layer and the second work function material layer includes a first atomic layer etching process; The first atomic layer etching process includes a single or multiple cycle process; Each cycle process includes: performing a first modification treatment on the surface to be etched to form a first modified layer; The first modified layer is removed.
5. The method for forming a semiconductor structure according to claim 4, It is characterized in that The modification process of the first work function material layer and the second work function material layer includes an oxidation process.
6. The method for forming a semiconductor structure according to claim 1, It is characterized in that The materials of the first work function material layer and the second work function material layer are P-type work function materials; or, the materials of the first work function material layer and the second work function material layer are N-type work function materials; the P-type work function material includes titanium nitride or tantalum nitride; the N-type work function material includes titanium aluminum.
7. The method for forming a semiconductor structure according to claim 1, It is characterized in that Before forming the first work function material layer on the substrate, the method also includes: forming a dielectric layer on the substrate; forming a first gate opening located on the first area in the dielectric layer; forming a second gate opening located on the second area in the dielectric layer, and forming a third gate opening located on the third area in the dielectric layer.
8. The method for forming a semiconductor structure according to claim 7, It is characterized in that Before forming the first work function material layer, the method further includes: forming a gate dielectric layer on the inner wall of the first gate opening, the inner wall of the second gate opening and the inner wall of the third gate opening; forming a protective layer on the gate dielectric layer, wherein the first work function material layer is located on the protective layer.
9. The method for forming a semiconductor structure according to claim 8, It is characterized in that After forming the protection layer, the method further includes: forming a stop layer on the protection layer, wherein the first work function material layer is located on the stop layer.
10. The method for forming a semiconductor structure according to claim 1, It is characterized in that After forming the fourth work function material layer, the method further includes: removing the fourth work function material layer on either one or both of the third and fourth regions.
11. The method for forming a semiconductor structure according to claim 10, It is characterized in that The process of removing the fourth work function material layer includes a second atomic layer etching process; The second atomic layer etching process includes a single or multiple cycle process; Each cycle process includes: performing a second modification treatment on the surface to be etched to form a second modified layer; The second modified layer is removed.
12. The method for forming a semiconductor structure according to claim 11, It is characterized in that The modification process for the fourth work function material layer includes an oxidation process.
13. The method for forming a semiconductor structure according to claim 1, It is characterized in that After forming the second work function structure and the third work function structure, the method further includes: forming a gate layer on the first region, the second region and the third region.