Non-aqueous electrolyte battery electrode binder, non-aqueous electrolyte battery electrode binder solution, non-aqueous electrolyte battery electrode slurry, non-aqueous electrolyte battery electrode and non-aqueous electrolyte battery

By using water-soluble resin with specific viscosity and thixotropic index as the electrode binder for non-aqueous electrolyte batteries, the problems of low viscosity and unstable active material settlement during the manufacturing process of the electrode binder are solved, and a high discharge capacity maintenance rate is achieved. and excellent peel strength.

CN113272997BActive Publication Date: 2024-10-29KURARAY CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202080008640.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-08
Publication Date
2024-10-29
Estimated Expiration
2040-01-08

AI Technical Summary

Technical Problem

During the manufacturing process, existing non-aqueous electrolyte battery electrode binders are prone to low viscosity, unstable active material settlement, and difficulty in uniform dispersion, resulting in poor electrode performance, especially insufficient discharge capacity maintenance and peeling strength.

Method used

A water-soluble resin with specific viscosity and thixotropic index is used as a non-aqueous electrolyte battery electrode binder. By adjusting the viscosity and thixotropic index of the aqueous solution, a uniform form is formed within the viscosity range at 10s-1 and 100s-1 shear rates. electrode to improve peel strength and discharge capacity maintenance rate.

Benefits of technology

It achieves the formation of uniform electrodes in non-aqueous electrolyte battery electrodes, improves peel strength and discharge capacity maintenance rate, reduces resistance, and enhances the stability and performance of the electrodes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a non-aqueous electrolyte battery electrode binder, which comprises a water-soluble resin, wherein the non-aqueous electrolyte battery electrode binder is in an aqueous solution state with a solid content concentration of 10% by mass, and the shear rate of the aqueous solution at 25° C. is 10s ‑1 The viscosity of the aqueous solution is 4 Pa·s or more and 30 Pa·s or less, and the shear rate of the aqueous solution at 25° C. is 10 s ‑1 The viscosity and shear rate at 100s ‑1 The thixotropic index defined by the viscosity ratio when the viscosity is 1.8 or more and 5 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-aqueous electrolyte battery electrode binder, a non-aqueous electrolyte battery electrode binder solution, a non-aqueous electrolyte battery electrode slurry, a non-aqueous electrolyte battery electrode and a non-aqueous electrolyte battery. Background Art

[0002] In recent years, portable terminals such as mobile phones, notebook personal computers, and handheld information terminals have become significantly popular. Portable terminals are required to be more comfortable to carry. With the rapid development of miniaturization, thinning, lightness, and high performance, the batteries used in portable terminals are also required to be miniaturized, thinned, lightened, and high-performance. As a secondary battery used in the power source of such portable terminals, lithium-ion secondary batteries are commonly used. Non-aqueous electrolyte batteries such as lithium-ion secondary batteries have the following structure: a positive electrode and a negative electrode are provided with a separator, and are contained in a container together with an electrolyte obtained by dissolving a lithium salt such as LiPF6, LiBF4, LiTFSI ((bistrifluoromethanesulfonyl imide) lithium), and LiFSI ((bisfluorosulfonyl imide) lithium) in an organic liquid such as ethylene carbonate.

[0003] The negative electrode and positive electrode constituting a non-aqueous electrolyte battery are usually formed as follows: a binder and a thickener are dissolved or dispersed in water or a solvent, an active material, a conductive aid (conductive imparting agent), etc. are mixed therein, the electrode slurry thus obtained is applied to a current collector, and the water or solvent is dried to form a mixed layer, which is then bonded.

[0004] From the perspective of reducing the burden on the environment and simplifying the manufacturing device, in particular, in the manufacture of the negative electrode, the electrode slurry using an aqueous medium is rapidly shifting. As such aqueous medium binders, known binders include vinyl alcohol polymers, acrylic acid and other acrylic acid polymers, and amide / imide polymer binders (e.g., Patent Documents 1 and 2).

[0005] On the other hand, in the manufacture of the positive electrode, an electrode slurry using a solvent is generally used. Examples of such solvents include organic solvents such as N-methyl-2-pyrrolidone, dimethylformamide, N,N-dimethylacetamide, N,N-dimethylmethanesulfonamide, and hexamethylphosphoric triamide. As a binder for such an organic solvent, a vinylidene fluoride polymer, a tetrafluoroethylene polymer, a fluororubber, and the like can be used (for example, Patent Documents 3 and 4).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 11-250915

[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-59527

[0010] Patent Document 3: Japanese Patent Application Publication No. 2017-107827

[0011] Patent Document 4: Japanese Patent Application Publication No. 2013-37955. Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, in the manufacture of either the negative electrode or the positive electrode, for the slurry obtained by mixing a binder, a solvent (water or a solvent) and an active material, a conductive aid (conductive imparting agent), etc., the form of materials such as the binder in the slurry and various conditions when preparing the slurry have an impact, and various problems may occur when applying it to a collector to form an electrode.

[0014] For example, the viscosity of the slurry prepared by containing vinyl alcohol polymers and water, which are generally used as negative electrode binders, is low, so the active material and the like are easily precipitated, and the slurry lacks stability. On the other hand, even when the slurry is made high in viscosity by increasing the molecular weight of the water-soluble resin in the slurry, the active material and the like in the slurry are difficult to disperse and it is difficult to uniformly form an electrode, so it is difficult to obtain sufficient performance, especially a high discharge capacity retention rate.

[0015] On the other hand, even if the slurry contains a vinylidene fluoride polymer mainly used as a positive electrode binder and an organic solvent, it is difficult to form a uniform electrode and maintain a suitable discharge capacity retention rate in the formed electrode due to the influence of its preparation conditions, as in the case where the solvent is water. On this basis, especially when using a slurry containing a commonly used vinylidene fluoride polymer to form an electrode (for example, Patent Documents 3 and 4), the adhesiveness of the binder to the metal foil in the electrode collector is weak, so the peel strength of the electrode becomes low, and thus, the active material in the electrode layer easily falls off from the metal foil.

[0016] Therefore, an object of the present invention is to provide a nonaqueous electrolyte battery electrode binder which, when used for a nonaqueous electrolyte battery electrode, can appropriately form a uniform electrode having excellent peel strength and a high discharge capacity retention rate.

[0017] Means used to solve problems

[0018] As a result of in-depth research conducted by the present inventors, it is known that when a non-aqueous electrolyte battery electrode binder containing a water-soluble resin is in a specified aqueous solution state, by making the aqueous solution have a viscosity within a specified range under specified conditions and a thixotropic index within a specified range under specified conditions, when the binder is used for an electrode, a uniform electrode can be appropriately formed, and the electrode can have excellent peel strength and a high discharge capacity retention rate.

[0019] That is, the present invention includes the following preferred embodiments.

[0020] [1] A non-aqueous electrolyte battery electrode binder comprising a water-soluble resin,

[0021] The non-aqueous electrolyte battery electrode binder is in the form of an aqueous solution with a solid content concentration of 10% by mass, and the shear rate of the aqueous solution at 25° C. is 10 s -1 The viscosity of the aqueous solution is 4 Pa·s or more and 30 Pa·s or less, and the shear rate of the aqueous solution at 25° C. is 10 s -1 The viscosity and shear rate at 100s -1 The thixotropic index defined by the viscosity ratio when the viscosity is 1.8 or more and 5 or less.

[0022] [2] The non-aqueous electrolyte battery electrode binder according to [1] above, wherein in the state of a solution of N-methyl-2-pyrrolidone having a solid content concentration of 7.5% by mass, the shear rate of the solution at 25° C. is 10 s -1 The viscosity of the solution is 4 Pa·s or more and 35 Pa·s or less, and the shear rate of the solution at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity at which the thixotropic index is defined as the viscosity ratio is 2 or more and 6 or less.

[0023] [3] The non-aqueous electrolyte battery electrode binder according to [1] or [2] above, wherein the water-soluble resin is a vinyl alcohol polymer having a cross-linked structure.

[0024] [4] A non-aqueous electrolyte battery electrode binder according to any one of [1] to [3] above, wherein the modification rate of the water-soluble resin is 0.02 mol % or more and 5 mol % or less based on the number of moles of all monomer units constituting the water-soluble resin.

[0025] [5] A non-aqueous electrolyte battery electrode binder solution comprising the non-aqueous electrolyte battery electrode binder described in any one of [1] to [4] above and water,

[0026] The shear rate of the non-aqueous electrolyte battery electrode binder solution at 25° C. is 10 s-1 The viscosity is 4 Pa·s or more and 30 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The thixotropic index defined by the viscosity ratio when the viscosity is 1.8 or more and 5 or less.

[0027] [6] A non-aqueous electrolyte battery electrode binder solution comprising the non-aqueous electrolyte battery electrode binder described in any one of [1] to [4] above and N-methyl-2-pyrrolidone,

[0028] The shear rate of the non-aqueous electrolyte battery electrode binder solution at 25° C. is 10 s -1 The viscosity is 4 Pa·s or more and 35 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity at which the thixotropic index is defined as the viscosity ratio is 2 or more and 6 or less.

[0029] [7] A non-aqueous electrolyte battery electrode slurry comprising the non-aqueous electrolyte battery electrode binder solution described in [5] or [6] above and an active material.

[0030] [8] The non-aqueous electrolyte battery electrode slurry according to [7] above, wherein the content of the non-aqueous electrolyte battery electrode binder is 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the active material.

[0031] [9] A non-aqueous electrolyte battery electrode comprising a solidified body of the non-aqueous electrolyte battery electrode slurry described in [7] or [8] above and a current collector.

[0032]

[10] A non-aqueous electrolyte battery comprising the non-aqueous electrolyte battery electrode described in [9] above.

[0033] Effects of the Invention

[0034] According to the present invention, it is possible to provide a non-aqueous electrolyte battery electrode binder which, when used for a non-aqueous electrolyte battery electrode, can appropriately form a uniform electrode having excellent peel strength and a high discharge capacity retention rate. DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described in detail. However, it should be noted that the present invention is not limited to the following embodiments.

[0036] <Non-aqueous electrolyte battery electrode binder>

[0037] The non-aqueous electrolyte battery electrode binder of the present invention (hereinafter also referred to as "the binder of the present invention" or "the binder") comprises a water-soluble resin, and in an aqueous solution state having a solid content concentration of 10% by mass (hereinafter also referred to as "the predetermined aqueous solution state"), the shear rate of the aqueous solution at 25° C. is 10 s -1 The viscosity at that time is 4 Pa·s or more and 30 Pa·s or less.

[0038] The binder is subjected to a predetermined aqueous solution at 25°C and a shear rate of 10 s. -1 The viscosity is 4 Pa·s or more, so that in the state of the non-aqueous electrolyte battery electrode slurry of the present invention (hereinafter also referred to as "the slurry of the present invention" or "slurry") described later, the adhesion between the solid body, especially the active material and the conductive additive that may be contained in the solid body, and the collector is improved, and an electrode with excellent peel strength can be formed. -1 When the viscosity is 30 Pa·s or less, the dispersibility of the active material and the like in the slurry can be maintained, and as a result, the effect of suppressing aggregation or sedimentation of the active material and the like is enhanced.

[0039] Furthermore, the slurry containing the binder of the present invention is stable, so it is not easy to produce unevenness when forming the non-aqueous electrolyte battery electrode of the present invention (hereinafter also referred to as "the electrode of the present invention" or "the electrode"), and the non-aqueous electrolyte battery of the present invention (hereinafter also referred to as "the battery of the present invention" or "the battery") finally obtained can maintain a high discharge capacity retention rate and reduce resistance.

[0040] The binder is in a specified aqueous solution at 25°C and a shear rate of 10s -1 The lower limit of the viscosity is preferably 4.1 Pa·s or more, more preferably 4.5 Pa·s or more, further preferably 5 Pa·s or more, further preferably 6 Pa·s or more, and further preferably 9 Pa·s or more. The binder is in a specified aqueous solution state at 25°C and a shear rate of 10 s -1 The upper limit of the viscosity at this time is preferably 29 Pa·s or less, more preferably 28.5 Pa·s or less, further preferably 28 Pa·s or less, and further preferably 27.5 Pa·s or less.

[0041] The binder of the present invention is in a specified aqueous solution state, and the shear rate of the aqueous solution at 25°C is 10s -1 The viscosity and shear rate at 100s -1 The viscosity ratio of the viscosity at shear rate of 10s -1 Viscosity / shear rate at 100s -1The thixotropic index (hereinafter also referred to as "TI") defined as the viscosity at the time of tackiness is 1.8 or more and 5 or less.

[0042] When the TI of the binder in a predetermined aqueous solution state is within the above range, a uniform electrode film can be formed when the slurry is applied to a current collector, and as a result, the discharge capacity retention rate of the finally obtained battery can be improved and the resistance can be reduced.

[0043] The lower limit of the TI defined by the viscosity ratio of the binder in a predetermined aqueous solution state is preferably 1.82 or more, more preferably 2 or more, further preferably 2.01 or more, further preferably 2.2 or more, and further preferably 2.22 or more. The upper limit of the TI defined by the viscosity ratio of the binder in a predetermined aqueous solution state is preferably 4.1 or less, more preferably 5 or less, further preferably 4 or less, and further preferably 3.5 or less.

[0044] In this specification, the solid content concentration in the solution can be calculated as follows: for example, a solution (ie, a solution containing a binder) is weighed into an aluminum cup, dried using a hot air dryer, and then the solid content mass remaining is calculated.

[0045] The binder of the present invention is in a solution state of N-methyl-2-pyrrolidone (hereinafter also referred to as "NMP") having a solid content concentration of 7.5 mass % (hereinafter also referred to as "specified NMP solution state"), and the shear rate of the solution at 25° C. is 10 s -1 The viscosity of the solution at 25°C may be 4 Pa·s or more and 35 Pa·s or less, and the shear rate of the solution at 25°C may be 10 s -1 The viscosity and shear rate at 100s -1 The viscosity at the time of TI defined by the viscosity ratio can be 2 or more and 6 or less.

[0046] The binder is subjected to a predetermined NMP solution state at 25°C and a shear rate of 10 s. -1 The viscosity of the binder is 4 Pa·s or more, so that in the slurry state with NMP as the solvent, the adhesion between the solidified body, especially the active material and the conductive additive that may be contained in the solidified body, and the collector is improved, and an electrode with extremely excellent peel strength can be formed. -1 When the viscosity is 35 Pa·s or less, the dispersibility of the active material and the like in the slurry using NMP as a solvent can be maintained, and as a result, the effect of suppressing aggregation or sedimentation of the active material and the like can be enhanced.

[0047] By setting the TI of the binder in a predetermined NMP solution state within the above range, a more uniform electrode can be produced when a slurry containing NMP as a solvent is applied to a current collector, and the discharge capacity retention rate of the finally obtained battery can be further improved.

[0048] The binder is in the specified NMP solution state at 25°C and a shear rate of 10s -1 The lower limit of the viscosity is preferably 4.5 Pa·s or more, more preferably 5 Pa·s or more, further preferably 8.5 Pa·s or more, and further preferably 15 Pa·s or more. The binder is in a specified NMP solution state at 25°C and a shear rate of 10 s -1 The upper limit of the viscosity at this time may be preferably 33 Pa·s or less, more preferably 27 Pa·s or less, and further preferably 24 Pa·s or less.

[0049] The lower limit of the TI defined by the viscosity ratio of the binder in a specified NMP solution state may be preferably 2.2 or more, more preferably 2.5 or more, and further preferably 2.7 or more. The upper limit of the TI defined by the viscosity ratio of the binder in a specified NMP solution state may be preferably 5.7 or less, more preferably 5 or less, further preferably 4.79 or less, and further preferably 3.2 or less.

[0050] In this specification, the binder is in a specified aqueous solution state or a specified NMP solution state at 25°C and a shear rate of 10 s -1 and 100s -1 The viscosity at the time of the reaction can be measured by using each solution as a measurement sample and using, for example, an E-type viscometer.

[0051] The viscosity and TI of the aqueous solution or NMP solution can be adjusted by appropriately changing the modification rate of the water-soluble resin, the viscosity average polymerization degree, various temperature conditions in the heating process of the water-soluble resin, the type and amount of other additives added to the binder, and the binder content in water or NMP.

[0052] The water-soluble resin in this specification can be any resin as long as it has solubility to dissolve more than 1g of the resin relative to 100g of water. For example, the water-soluble resin can include vinyl alcohol polymers and derivatives thereof, acrylic acid polymers such as (meth) acrylic acid and derivatives thereof, cellulose derivatives such as carboxymethyl cellulose, alginic acid and neutralized products thereof, polyvinyl pyrrolidone, etc., but is not limited to them.

[0053] Among these, the water-soluble resin is preferably a vinyl alcohol polymer and its derivatives. This is because: the vinyl alcohol polymer (also referred to as "polyvinyl alcohol" or "PVA" in this specification) has good affinity for active materials used in non-aqueous electrolyte batteries such as carbon materials, metals, and metal oxides. The water-soluble resin is more preferably PVA with a cross-linked structure. This is because: by having a cross-linked structure, it is easy to control the viscosity and TI of the binder in a specified aqueous solution state to within the specified range as described above.

[0054] The method for forming the cross-linked structure of PVA is not particularly limited. Examples of the method include a method of heat-treating PVA under a nitrogen or air atmosphere, a method of acid-treating unmodified PVA, and a method of chemically cross-linking using a multifunctional additive. Alternatively, a modified PVA capable of pre-constructing a cross-linked structure may be used.

[0055] Acidic substances that can be used in the method of acid-treating unmodified PVA include inorganic acids such as acetic acid, hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid; organic acids such as formic acid, acetic acid, oxalic acid and p-toluenesulfonic acid; salts such as pyridinium p-toluenesulfonate and ammonium chloride; Lewis acids such as zinc chloride, aluminum chloride, ferric chloride, tin dichloride, tin tetrachloride and boron trifluoride diethyl ether complex, etc. Among these, one or more kinds can be used in combination. The amount of these acidic substances is preferably 0.0001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of PVA.

[0056] The polyfunctional additives that can be used in the method of chemical crosslinking using a polyfunctional additive can be dialdehydes such as glyoxal and 1,4-butanedialdehyde; diepoxides such as ethylene glycol diglycidyl ether and diethylene glycol diglycidyl ether; diisocyanates such as hexamethylene diisocyanate and toluene diisocyanate, etc. The amount of these polyfunctional additives is preferably 0.0001 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of PVA.

[0057] As PVA, PVA obtained by saponifying a vinyl ester polymer can be used.

[0058] The vinyl ester monomer used in the production of the vinyl ester polymer is not particularly limited, and examples thereof include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl versatate, vinyl caproate, vinyl octanoate, vinyl laurate, vinyl palmitate, vinyl stearate, vinyl oleate, vinyl benzoate, etc. Among these, vinyl acetate is preferred from an economical point of view.

[0059] PVA may be unmodified PVA consisting only of vinyl alcohol units, but preferably further contains units derived from monomer (a). PVA having a crosslinked structure is produced by heating a polymer consisting of vinyl alcohol monomer and monomer (a) to form ester bonds, thereby crosslinking.

[0060] The monomer (a) may be at least one monomer selected from the group consisting of a carboxylic acid having an unsaturated double bond, an alkyl ester of the carboxylic acid, an anhydride of the carboxylic acid, a salt of the carboxylic acid, and a silyl compound having an unsaturated double bond.

[0061] Examples of the carboxylic acid having an unsaturated double bond, the alkyl ester of the carboxylic acid, the anhydride of the carboxylic acid, and the salt of the carboxylic acid include maleic acid, monomethyl maleate, dimethyl maleate, monoethyl maleate, diethyl maleate, maleic anhydride, citraconic acid, monomethyl citraconic acid, dimethyl citraconic acid, diethyl citraconic acid, citraconic anhydride, fumaric acid, monomethyl fumarate, dimethyl fumarate, monoethyl fumarate, diethyl fumarate, itaconic acid, monomethyl itaconate, dimethyl itaconate, monoethyl itaconate, diethyl itaconate, itaconic anhydride, acrylic acid, methyl acrylate, ethyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, and the like.

[0062] Examples of the silyl compound having an unsaturated double bond include compounds having an unsaturated double bond and a trialkoxysilyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane.

[0063] Among these monomers (a), preferred are monomethyl maleate, dimethyl maleate, monomethyl citraconic acid, monomethyl fumarate, monomethyl itaconate, itaconic anhydride, methyl acrylate, methyl methacrylate, and vinyltrimethoxysilane, and more preferred are monomethyl maleate, dimethyl maleate, monomethyl fumarate, itaconic anhydride, methyl acrylate, methyl methacrylate, and vinyltrimethoxysilane.

[0064] The modification rate of the water-soluble resin is preferably 0.02 mol% or more and 5 mol% or less based on the molar number of all monomer units constituting the water-soluble resin. It should be noted that the modification rate of the water-soluble resin refers to the content of units derived from the monomer (a) based on the molar number of all monomer units constituting the water-soluble resin.

[0065] The lower limit of the modification rate is more preferably 0.05 mol %, further preferably 0.1 mol %, and further preferably 0.2 mol %. The upper limit of the modification rate is more preferably 4.5 mol %, further preferably 3 mol %, and further preferably 1.1 mol %.

[0066] The modification rate of the water-soluble resin can be determined by using a vinyl ester polymer as a water-soluble resin, such as a PVA precursor, as described in the examples below. 1 It was determined by the H-NMR method.

[0067] By setting the modification rate to be greater than or equal to 0.02 mol % and less than or equal to 5 mol %, the viscosity and TI of the binder containing a water-soluble resin in a solution state can be easily adjusted to within a predetermined range, and the adhesion of the adhesive layer formed from the slurry containing the binder containing a water-soluble resin can be further improved.

[0068] Specifically, if the modification rate of the water-soluble resin is improved, the viscosity and TI of the solution in the prescribed aqueous solution state or the prescribed NMP solution state will increase. By setting the modification rate to less than 5 mol%, the viscosity and TI in the prescribed aqueous solution state and the prescribed NMP solution can be maintained within the prescribed range without excessively increasing it, and the solubility of the water-soluble resin in water or NMP can be made more excellent. In addition, the slurry prepared by the binder of the present invention can be stabilized, and the worry of aggregation of the active material in the slurry can be further reduced, and a uniform electrode can be formed more suitably. Therefore, the battery of the present invention finally manufactured can be constituted in a manner with lower resistance and higher discharge capacity maintenance rate. On the other hand, by setting the modification rate to more than 0.02 mol%, the viscosity can not be excessively reduced, and an electrode with excellent adhesion can be formed.

[0069] The water-soluble resin, especially PVA, may contain units derived from other monomers in addition to the vinyl alcohol unit and the unit derived from the monomer (a) within a range that does not impair the effect of the present invention. As the units derived from other monomers, for example, units derived from α-olefins such as ethylene, propylene, n-butene and isobutylene, vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether and 2,3-diacetoxy-1-vinyloxypropane, vinyl cyanides such as acrylonitrile and methacrylonitrile, vinyl halides such as vinyl chloride and vinyl fluoride, vinylidene halides such as vinylidene chloride and vinylidene fluoride, allyl acetate, allyl compounds such as 2,3-diacetoxy-1-allyloxypropane and allyl chloride, and isopropenyl acetate, etc. The content of the units derived from other monomers in the water-soluble resin, especially PVA, can be set to, for example, 15 mol% or less based on the molar number of all monomer units constituting the water-soluble resin.

[0070] The arrangement order of the vinyl alcohol units, the units derived from the monomer (a), and the units derived from the other monomers in the water-soluble resin, especially PVA, is not particularly limited, and may be any of random, block, and alternating.

[0071] It should be noted that the primary structure of the water-soluble resin can be 1 Quantitative analysis was performed by H-NMR.

[0072] The lower limit of the saponification degree (the molar fraction of the hydroxyl group in the water-soluble resin relative to the total of the hydroxyl group and the ester bond) in the water-soluble resin, especially PVA, is preferably 20 mol% or more, more preferably 60 mol% or more, further preferably 70 mol% or more, further preferably 75 mol% or more, and further preferably 80 mol% or more. The saponification degree can be measured in accordance with JIS-K6726:1994 as in the examples described below.

[0073] The upper limit of the viscosity average polymerization degree of the water-soluble resin, especially PVA, is preferably 5000 or less, more preferably 4000 or less. On the other hand, the lower limit of the viscosity average polymerization degree of the water-soluble resin is preferably 100 or more, more preferably 500 or more, and further preferably 1000 or more. It should be noted that when the water-soluble resin has a cross-linked structure, the viscosity average polymerization degree of the water-soluble resin before cross-linking is preferably within the aforementioned range. If the viscosity average polymerization degree of the water-soluble resin is large, the viscosity of the solution in a prescribed aqueous solution state or a prescribed NMP solution state will increase. In addition, if the viscosity average polymerization degree of the water-soluble resin is large, the TI of the solution in a prescribed aqueous solution state or a prescribed NMP solution state can be easily adjusted to a prescribed range. By making the viscosity average polymerization degree of the water-soluble resin greater than 100, the viscosity and TI of the binder containing the water-soluble resin in the aqueous solution or NMP solution state can be easily adjusted to a prescribed range without excessively reducing it, and the adhesion of the adhesive layer formed by the slurry containing the binder containing the water-soluble resin can be improved. On the other hand, by setting the viscosity average degree of polymerization of the water-soluble resin to 5000 or less, the viscosity and TI in the aqueous solution or NMP solution state will not increase excessively, and the productivity of the water-soluble resin will be improved, so that the water-soluble resin can be produced at a lower cost.

[0074] The viscosity average polymerization degree (P) of the water-soluble resin can be calculated as follows: After the water-soluble resin is completely saponified and purified, the intrinsic viscosity [η] (unit: liter / g) of the water-soluble resin containing units derived from the monomer (a) is measured in a 30°C sodium chloride aqueous solution (0.5 mol / L), and the intrinsic viscosity [η] (unit: liter / g) of the water-soluble resin not containing units derived from the monomer (a) is measured in a 30°C aqueous solution. The viscosity average polymerization degree (P) of the water-soluble resin is calculated from the intrinsic viscosity [η] by the following formula.

[0075] P=([η]×104 / 8.29)(1 / 0.62)

[0076] Hereinafter, an example of a method for producing PVA, which is one of water-soluble resins, will be described.

[0077] The process of manufacturing PVA includes, for example, a process of polymerizing monomers including vinyl ester monomers (hereinafter also referred to as "polymerization process"), and a process of saponifying the vinyl ester polymer obtained by the polymerization process (hereinafter also referred to as "saponification process"). Preferably, the process further includes a process of heating the vinyl ester polymer or the saponified PVA (hereinafter also referred to as "heating process").

[0078] In the polymerization step, monomers including vinyl ester monomers are polymerized to synthesize vinyl ester polymers. The monomers used in the polymerization step may be only vinyl ester monomers, or may include vinyl ester monomers and monomer (a) and / or other monomers as described above.

[0079] The polymerization method of the monomer containing the vinyl ester monomer may be any of batch polymerization, semi-batch polymerization, continuous polymerization and semi-continuous polymerization. The polymerization method may adopt any known method such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. Among these, bulk polymerization or solution polymerization in which polymerization is carried out in a solvent-free state or in a solvent such as alcohol is generally adopted. When obtaining a vinyl ester polymer with a high degree of polymerization, an emulsion polymerization method may be adopted. The solvent for the solution polymerization method is not particularly limited, and examples thereof include alcohols. The alcohol used as the solvent for the solution polymerization method is, for example, a lower alcohol such as methanol, ethanol, and n-propanol. The solvent may be used alone or in combination of two or more. The amount of solvent used in the polymerization system may be selected according to the degree of polymerization of the target PVA, etc., taking into account the chain transfer of the solvent. For example, when the solvent is methanol, the lower limit of the mass ratio {= (solvent) / (total monomers)} of the solvent to all monomers contained in the polymerization system is preferably 0.01 or more, and more preferably 0.05 or more. On the other hand, the upper limit of the mass ratio is preferably 10 or less, and more preferably 3 or less.

[0080] The polymerization initiator used for the polymerization can be appropriately selected from known polymerization initiators such as azo initiators, peroxide initiators, redox initiators, etc. according to the polymerization method. Examples of azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). Examples of peroxide initiators include percarbonate compounds such as diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and diethoxyethyl peroxydicarbonate; perester compounds such as tert-butyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, and tert-butyl peroxyneodecanoate; acetyl peroxide, acetylcyclohexylsulfonyl peroxide, and 2,4,4-trimethylpentyl-2-peroxyphenoxyacetate. Furthermore, these initiators can be combined with potassium persulfate, ammonium persulfate, hydrogen peroxide, etc. as an initiator. As the redox initiator, for example, an initiator obtained by combining the above-mentioned peroxide initiator with a reducing agent such as sodium bisulfite, sodium bicarbonate, tartaric acid, L-ascorbic acid, Rongalite, etc. can be cited.

[0081] The amount of the polymerization initiator used varies depending on the polymerization catalyst, etc., and cannot be generalized. For example, it can be appropriately selected according to the polymerization rate. For example, when 2,2'-azobisisobutyronitrile or acetyl peroxide is used as the polymerization initiator, the lower limit of the amount of the polymerization initiator used is preferably 0.01 mol% or more, and more preferably 0.02 mol% or more relative to the vinyl ester monomer. On the other hand, the upper limit of the amount of the polymerization initiator used is preferably 0.2 mol% or less, and more preferably 0.15 mol% or less.

[0082] The lower limit of the temperature in the polymerization process is preferably above 0°C, more preferably above 30°C. The upper limit of the polymerization temperature is preferably below 200°C, more preferably below 140°C. By setting the polymerization temperature to above 0°C, the polymerization rate can be increased. On the other hand, by setting the polymerization temperature to below 200°C, it is easy to maintain the content of units derived from monomer (a) in the water-soluble resin to an appropriate ratio even when, for example, monomer (a) is used. Methods for controlling the polymerization temperature within the above range include, for example, a method of balancing the heat generated by the polymerization and the heat released from the reactor surface by controlling the polymerization rate; a method of controlling by using an external jacket using an appropriate heat medium, etc. From the perspective of safety, the latter method is preferred.

[0083] The polymerization can be carried out in the presence of a chain transfer agent within the range that does not impair the effect of the present invention. Examples of chain transfer agents include aldehydes such as acetaldehyde and propionaldehyde; ketones such as acetone and methyl ethyl ketone; thiols such as 2-hydroxyethanethiol; halogenated hydrocarbons such as trichloroethylene and perchloroethylene; and phosphinates such as sodium phosphinate monohydrate. Among these, aldehydes and ketones are preferred. The amount of chain transfer agent added to the polymerization system can be determined based on the chain transfer coefficient of the added chain transfer agent and the degree of polymerization of the target water-soluble resin. Generally speaking, it is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the vinyl ester monomer.

[0084] When polymerization is performed at high temperature, for example, when PVA is used as a water-soluble resin, coloration of PVA due to decomposition of vinyl ester monomers is sometimes observed. In this case, an antioxidant such as tartaric acid may be added to the polymerization system in an amount of about 1 ppm to 100 ppm relative to the vinyl ester monomer to prevent coloration.

[0085] In the saponification step, for example, when PVA is used as the water-soluble resin, the vinyl ester polymer is saponified. By saponifying the polymer, the vinyl ester unit in the polymer is converted into a vinyl alcohol unit.

[0086] The reaction used for saponification is not particularly limited, and for example, a known alcoholysis reaction or hydrolysis reaction performed in a state where a vinyl ester polymer is dissolved in a solvent can be used.

[0087] Examples of the solvent used for saponification include lower alcohols such as methanol and ethanol; esters such as methyl acetate and ethyl acetate; ketones such as acetone and methyl ethyl ketone; and aromatic hydrocarbons such as benzene and toluene. These solvents may be used alone or in combination of two or more. Among these, methanol and a mixed solution of methanol and methyl acetate are preferred.

[0088] Catalysts used for saponification include base catalysts such as alkali metal hydroxides (potassium hydroxide, sodium hydroxide, etc.) and sodium alkoxides (sodium methoxide, etc.); and acid catalysts such as p-toluenesulfonic acid and inorganic acids. Among these, sodium hydroxide is preferred because of its ease of use.

[0089] The temperature for saponification is not particularly limited, but is preferably 20° C. to 60° C. When a gel-like product is gradually precipitated as the saponification proceeds, the product can be crushed and further saponified. Thereafter, the saponification is terminated by neutralizing the resulting solution, and the saponification is washed and dried to obtain a water-soluble resin. The saponification method is not limited to the above method, and other known methods can be used.

[0090] In the heating process, for example, when PVA is used as a water-soluble resin, a vinyl ester polymer or PVA is heated. Specifically, the vinyl ester polymer is heated by heating simultaneously with the saponification process, or the obtained PVA is heated after the saponification process is completed. By this heating, it is easy to obtain a PVA with a cross-linked structure. The higher and longer the heating temperature, the more cross-linked structures are formed, and the viscosity will increase. By adjusting the conditions of this heating process, the viscosity of the binder containing PVA in a solution state can be easily adjusted to a specified range, and the adhesion of the adhesive layer formed by the slurry containing the binder containing PVA is further improved. The heat treatment is preferably carried out under air or nitrogen atmosphere. In addition, the heating process is preferably carried out after saponification.

[0091] The lower limit of the heating temperature in the heating process is preferably 70°C or more, more preferably 90°C or more. The upper limit of the heating temperature is preferably 170°C or less, more preferably 150°C or less. The lower limit of the heating time in the heating process is preferably 30 minutes or more, more preferably 1 hour or more, and more preferably 2 hours or more. The upper limit of the heating time is preferably 10 hours or less, more preferably 7 hours or less, and more preferably 5 hours or less. If the heating temperature is increased or the heating time is extended, the viscosity and TI in the prescribed aqueous solution state or NMP solution state will increase. By setting the heating temperature to 170°C or less and / or the heating time to 10 hours or less, the generation of insoluble components can be prevented when it is subsequently dissolved in water or NMP.

[0092] The binder of the present invention may also contain a material to adjust the viscosity of the binder in the aqueous solution state or the NMP solution state. As the material for adjusting the viscosity, inorganic substances such as polyacids and salts thereof, condensates thereof, fumed silica, and alumina such as citric acid, tartaric acid, and aspartic acid may be cited. Their addition is not particularly limited, and usually relative to 100 mass parts of PVA, preferably more than 0.01 mass part and less than 10 mass parts, more preferably more than 0.02 mass part and less than 8 mass parts, and further preferably more than 0.05 mass part and less than 5 mass parts. The more the content of the material for adjusting the viscosity is, the more the viscosity and TI of the binder of the present invention in the solution state can be increased, and it is possible to more easily adjust to the specified range. The smaller the particle size of the inorganic substance contained, the easier it is to increase the viscosity and TI of the binder in the aqueous solution state or the NMP solution state.

[0093] The binder of the present invention or the non-aqueous electrolyte battery electrode binder solution of the present invention described later can further contain a compounding agent within the scope of not damaging the effect of the present invention. As a compounding agent, for example, light stabilizers, ultraviolet absorbers, freeze stabilizers, thickeners, leveling agents, rheological stabilizers, thixotropic agents, defoamers, plasticizers, lubricants, preservatives, rust inhibitors, antistatic agents, anti-charge agents, anti-yellowing agents, pH regulators, film-forming aids, curing catalysts, cross-linking reaction catalysts, cross-linking agents (glyoxal, urea resins, melamine resins, polyvalent metal salts, polyisocyanates, polyamide epichlorohydrin, etc.), dispersants, etc. can be listed. Can be selected or combined according to their respective purposes to mix. The content of the compounding agent is based on the total amount of the binder or the non-aqueous electrolyte battery electrode binder solution, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less.

[0094] The binder of the present invention can be obtained by dissolving a water-soluble resin, especially PVA, and components other than the water-soluble resin as required in a solvent (water or NMP) to form a solution, and removing the solvent. In addition, the solution can also be directly used as a non-aqueous electrolyte battery electrode binder solution of the present invention described later and then used to prepare a slurry. At this time, the composition of the components other than the solvent in the binder solution is the binder of the present invention. The binder of the present invention is included in the cured body of the slurry composition of the present invention in a state mixed with components such as active materials.

[0095] <Non-aqueous electrolyte battery electrode binder solution>

[0096] The non-aqueous electrolyte battery electrode binder solution of the present invention (hereinafter also referred to as "binder solution" or "binder solution of the present invention") is a non-aqueous electrolyte battery electrode binder solution comprising the aforementioned binder of the present invention and water, and the shear rate at 25°C is 10s -1 The viscosity is 4 Pa·s or more and 30 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity ratio of the viscosity when the TI is defined is 1.8 or more and 5 or less. That is, the binder aqueous solution includes not only a binder aqueous solution having a solid content concentration of 10 mass %, but also a binder aqueous solution having a solid content concentration within a specific range that can satisfy the viscosity range under the above conditions and the TI range under the above conditions.

[0097] Alternatively, another non-aqueous electrolyte battery electrode binder solution of the present invention is a non-aqueous electrolyte battery electrode binder solution comprising the aforementioned binder of the present invention and N-methyl-2-pyrrolidone, wherein the shear rate at 25° C. is 10 s -1The viscosity is 4 Pa·s or more and 35 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity ratio of the viscosity at the time of the reaction is defined as TI of 2 or more and 6 or less. That is, the binder NMP solution includes not only a binder NMP solution having a solid content concentration of 7.5% by mass, but also a binder NMP solution having a solid content concentration within a specific range that can satisfy the viscosity range under the aforementioned conditions and the TI range under the aforementioned conditions.

[0098] As described above, the binder solution of the present invention comprises the binder of the present invention and at least one solvent. The solvent is water or NMP. When the solvent is water, it is suitable from the viewpoint of reducing environmental burden and simplicity of equipment. On the other hand, when the solvent is NMP, especially when used as a positive electrode slurry, it will not deteriorate the active material in the slurry, so it is suitable.

[0099] In addition to the binder of the present invention, the binder solution may contain an additive (referred to as additive A) that is soluble in the solvent within a range that does not impair the effects of the present invention. Examples of additive A include polyethylene glycol, polyethylene glycol dimethyl ether, polyethylene glycol diglycidyl ether, and polyethyleneimine. The content of additive A is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less, based on the total amount of the binder solution. It is particularly preferred that additive A is not contained.

[0100] The binder solution is obtained by mixing a water-soluble resin such as PVA, a solvent (water or NMP) and components other than the aqueous solution resin as described above as required by a known method such as stirring. The mixing temperature and mixing time can be appropriately adjusted according to the type of solvent. It should be noted that the binder solution refers to a solution in which the water-soluble resin is dissolved in a solvent. The dissolved state refers to a water-soluble resin that is completely dissolved in a solvent, especially a state in which the mass of PVA is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, further preferably 99% by mass or more, and further preferably 100% by mass relative to the total mass (100% by mass) of the water-soluble resin used when making the binder solution.

[0101] The content of the water-soluble resin, especially PVA, in the binder solution of the present invention is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and particularly preferably 5% by mass or more and 15% by mass or less based on the total amount of the binder solution. If the content of the water-soluble resin is 1% by mass or more, it is easy to improve the adhesion of the active material to the collector when forming an electrode. If the content of the water-soluble resin is 30% by mass or less, it is possible to suppress the rapid aggregation of the active material when forming an electrode.

[0102] <Non-aqueous electrolyte battery electrode slurry>

[0103] The non-aqueous electrolyte battery electrode slurry of the present invention comprises the aforementioned binder solution of the present invention and an active material.

[0104] The slurry of the present invention can be used for any electrode of the positive electrode and the negative electrode. In addition, it can also be used for both the positive electrode and the negative electrode. Therefore, the active material can be any one of the positive electrode active material and the negative electrode active material. Preferably, when the binder solution of the present invention contains water (when the solvent is water), it contains the negative electrode active material and is used as a slurry for the negative electrode. Preferably, when the binder solution of the present invention contains NMP (when the solvent is NMP), it contains the positive electrode active material and is used as a slurry for the positive electrode.

[0105] The negative electrode active material may be a material that has been used as a negative electrode active material for non-aqueous electrolyte batteries. Examples thereof include carbonaceous materials such as amorphous carbon, artificial graphite, natural graphite (graphite), mesocarbon microbeads (MCMB), pitch-based carbon fibers, carbon black, activated carbon, carbon fibers, hard carbon, soft carbon, mesoporous carbon, and conductive polymers such as polyacene; SiO x SnO x and LiTiO x The composite metal oxides shown, other metal oxides, lithium metals, lithium alloys and other lithium-based metals; metal compounds such as TiS2 and LiTiS2; and composite materials of metal oxides and carbonaceous materials. Among these, graphite is preferred, and spherical natural graphite is particularly preferred from the viewpoint of economy and battery capacity. These negative electrode active materials can be used alone or in combination of two or more.

[0106] The positive electrode active material may be a material that has been used as a positive electrode active material for non-aqueous electrolyte batteries. Examples thereof include TiS2, TiS3, amorphous MoS3, Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, and V6O. 13and lithium-containing composite metal oxides such as LiCoO2, LiNiO2, LiMnO2, and LiMn2O4. These positive electrode active materials can be used alone or in combination of two or more.

[0107] The slurry may include a conductive aid. The conductive aid is used to make the nonaqueous electrolyte battery realize high output, and is appropriately selected according to the occasion for the positive electrode or the negative electrode. As its example, for example, graphite, acetylene black, carbon black, Ketjen black, vapor-grown carbon fiber, etc. can be listed. From the viewpoint of the high output of the obtained nonaqueous electrolyte battery, acetylene black is preferably used among these.

[0108] When the slurry contains a conductive auxiliary agent, the content of the conductive auxiliary agent is preferably 0.1 mass parts or more and 15 mass parts or less, more preferably 1 mass parts or more and 10 mass parts or less, and further preferably 3 mass parts or more and 10 mass parts or less relative to 100 mass parts of the active material. If the content of the conductive auxiliary agent is within this range, the battery capacity to which the slurry is applied will not be reduced, and a sufficient conductive auxiliary effect can be obtained.

[0109] The content of the binder in the slurry is preferably 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the active material. If the content is 0.1 parts by mass or more, the adhesion of the active material to the collector is improved, which is beneficial from the viewpoint of maintaining the durability of the applied battery. Furthermore, if the content is 20 parts by mass or less, the discharge capacity is easily improved. The range of the content is more preferably 0.2 parts by mass or more and 18 parts by mass or less, more preferably 0.5 parts by mass or more and 16 parts by mass or less, and more preferably 1 part by mass or more and 12 parts by mass or less.

[0110] In addition to the binder, active material, conductive additive and solvent, the slurry may contain additives such as flame retardant, thickener, defoamer, leveling agent, adhesion agent, etc. as needed. When these additives are included, the content of the additives is preferably about 0.1% by mass or more and 10% by mass or less based on the total amount of the slurry.

[0111] The slurry can be obtained by mixing a binder, an active material, and, if necessary, a conductive auxiliary agent, a solvent, and additives by a conventional method, for example, using a mixer such as a ball mill, a blending mill, or a three-roll mill.

[0112] <Non-aqueous electrolyte battery electrode>

[0113] The nonaqueous electrolyte battery electrode of the present invention comprises a solidified body of the slurry of the present invention and a current collector. The solidified body of the slurry is a solidified product obtained by removing the solvent in the slurry by drying or the like.

[0114] In the electrode (positive electrode and negative electrode) of the present invention, the active material has excellent adhesion to the collector. Therefore, the peel strength of the electrode is preferably 30N / m or more, more preferably 50N / m or more, further preferably 60N / m or more, and particularly preferably 70N / m or more before being impregnated with the electrolyte. In particular, in the case of the positive electrode, the adhesion is more excellent, and the peel strength is preferably 300N / m or more, more preferably 500N / m or more, further preferably 600N / m or more, and particularly preferably 700N / m or more. It should be noted that the upper limit of the peel strength of the electrode is 1000N / m or less.

[0115] The electrode can be obtained by applying the slurry of the present invention to a current collector and removing the solvent by drying, etc. Furthermore, the electrode may be subjected to a rolling treatment after drying.

[0116] The current collector is not particularly limited as long as it contains a conductive material. Examples include metal materials such as iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. These current collectors can be used alone or in combination of two or more. Among the current collectors, from the viewpoint of the adhesion and discharge capacity of the active material, copper is preferably used as the negative electrode collector, and aluminum is preferably used as the positive electrode collector.

[0117] The method for applying the slurry to the current collector is not particularly limited, and examples thereof include an extrusion coater, a reverse roll, a doctor blade, an applicator, etc. The amount of the slurry applied is appropriately selected depending on the desired thickness of a cured product derived from the slurry composition.

[0118] Examples of the rolling method for the electrode include die pressing, roll pressing, etc. The pressing pressure is preferably 1 MPa or more and 40 MPa or less from the viewpoint of easily increasing the battery capacity.

[0119] In the electrode of the present invention, the thickness of the current collector is preferably 1 μm to 20 μm, more preferably 2 μm to 15 μm. The thickness of the solidified body is preferably 10 μm to 400 μm, more preferably 20 μm to 300 μm. The thickness of the electrode is preferably 20 μm to 200 μm.

[0120] <Non-aqueous electrolyte battery>

[0121] The nonaqueous electrolyte battery of the present invention includes the nonaqueous electrolyte battery electrode of the present invention as a negative electrode and / or a positive electrode.

[0122] Examples of the battery of the present invention include lithium ion batteries, sodium ion batteries, lithium sulfur batteries, all-solid batteries, lithium ion capacitors, and lithium batteries.

[0123] The battery of the present invention has a high discharge capacity and can maintain its discharge capacity even after repeated charge and discharge. The capacity retention rate (discharge capacity retention rate) of the battery of the present invention is preferably 80% or more, more preferably 90% or more, further preferably 95% or more, further preferably 98% or more, and further preferably 99% or more.

[0124] It should be noted that the discharge capacity retention rate of the battery can be calculated by, for example, a method of performing a charge and discharge test using a commercially available charge and discharge tester as described in the Examples below.

[0125] The electrolyte contained in the battery is a solution obtained by dissolving an electrolyte in a solvent. The electrolyte can be any electrolyte used in a conventional non-aqueous electrolyte battery, and can be in a liquid or gel state. A substance that can function as a battery can be appropriately selected according to the types of the negative electrode active material and the positive electrode active material. As a specific electrolyte, for example, well-known lithium salts can be suitably used, and examples thereof include LiClO4, LiBF6, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiB(C2H5)4, CF3SO3Li, CH3SO3Li, LiCF3SO3, LiC4F9SO3, Li(CF3SO2)2N, lower aliphatic carboxylic acid lithium, etc.

[0126] The solvent contained in the electrolyte is not particularly limited. Specific examples thereof include carbonates such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and vinylene carbonate; lactones such as γ-butyrolactone; ethers such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, and 2-methyltetrahydrofuran; sulfoxides such as dimethyl sulfoxide; tetrahydrofurans such as 1,3-dioxolane and 4-methyl-1,3-dioxolane. Furans; nitrogen-containing compounds such as acetonitrile and nitromethane; organic acid esters such as methyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate and ethyl propionate; inorganic acid esters such as triethyl phosphate, dimethyl carbonate and diethyl carbonate; diethylene glycol dimethyl ether and triethylene glycol dimethyl ether; oxazolidinones such as cyclopentane sulfone and 3-methyl-2-oxazolidinone; sultones such as 1,3-propane sultone, 1,4-butane sultone and naphthalene sultone, etc. They can be used alone or in combination of two or more. When using a gel electrolyte, a nitrile polymer, an acrylic polymer, a fluorine polymer, an alkylene oxide polymer, etc. can be added as a gelling agent.

[0127] When the electrode of the present invention is used for either the positive electrode or the negative electrode, a conventional electrode may be used as the electrode other than the electrode of the present invention.

[0128] In a preferred embodiment, the battery of the present invention includes the electrode of the present invention as a negative electrode and includes a conventional electrode as a positive electrode. The positive electrode is not particularly limited as long as it is a positive electrode commonly used in nonaqueous electrolyte batteries.

[0129] Alternatively, in another preferred embodiment, the battery of the present invention comprises the electrode of the present invention as a positive electrode and comprises a conventional electrode as a negative electrode. The negative electrode is not particularly limited as long as it is a negative electrode commonly used in non-aqueous electrolyte batteries. At this time, the binder solution of the present invention contained in the slurry of the present invention used to form the positive electrode is a binder solution containing the binder of the present invention and N-methyl-2-pyrrolidone, preferably: its shear rate at 25°C is 10s -1 The viscosity of the solution is 4 Pa·s or more and 35 Pa·s or less, and the shear rate of the solution at 25°C is 10s -1 The viscosity and shear rate at 100s -1 The viscosity ratio of the viscosity at the time is defined as TI of 2 or more and 6 or less. This is because: by making the solvent in the slurry NMP, the degradation of the positive electrode active material in the slurry is prevented, and by making the viscosity and TI of the binder NMP solution under the above conditions respectively within the above specified ranges, the peel strength of the positive electrode can be further improved.

[0130] Furthermore, both the positive electrode and the negative electrode may be electrodes containing the binder of the present invention.

[0131] The method for manufacturing the battery of the present invention is not particularly limited, and for example, it can be manufactured as follows. That is, the negative electrode and the positive electrode are overlapped with a separator such as a polypropylene porous film, and are rolled and / or folded according to the shape of the battery, and placed in a battery container, and an electrolyte is injected and sealed. The battery shape can be any one of a known coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.

[0132] The battery of the present invention is useful in various applications. For example, it is also very useful as a battery used in a portable terminal requiring miniaturization, thinning, lightening, and high performance. In addition, it can also be suitably used in batteries for devices requiring flexibility, such as wound-type dry batteries and laminated batteries. Example

[0133] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited thereto. The % in the examples refers to mass unless otherwise specified. First, the determination method and the evaluation method are shown below. It should be noted that the physical property values ​​(or evaluation values) recorded in this specification are based on the values ​​obtained by the following methods.

[0134] The physical properties of each PVA used in each of the examples and comparative examples described below, the evaluation of the binder aqueous solution and NMP solution containing the PVA, the evaluation of the negative electrode slurry, the evaluation in electrode application, and the evaluation in battery application were measured according to the following methods.

[0135] <Modification rate of PVA in binder>

[0136] The modification ratio of PVA used in each of the examples and comparative examples described below (the content ratio of the unit derived from the monomer (a) based on the number of moles of all monomer units of each PVA) was determined by using a vinyl ester polymer as a precursor of each PVA and 1 It was determined by the H-NMR method.

[0137] <Saponification Degree of PVA in Binder>

[0138] The saponification degree of PVA used in each of the examples and comparative examples described below was determined in accordance with JIS-K6726:1994.

[0139] <Polymerization Degree of PVA in Binder>

[0140] The degree of polymerization (viscosity average degree of polymerization) of PVA used in each of the examples and comparative examples described below was determined by the method described in JIS-K6726:1994.

[0141] For example, when monomethyl maleate is used as monomer (a), the above content is obtained by the following steps. That is, the vinyl ester polymer as a precursor of PVA is fully reprecipitated and purified three or more times using n-hexane / acetone as a solvent, and the obtained purified product is dried under reduced pressure at 50°C for 2 days to prepare a sample for analysis. The sample is dissolved in CDCl3 and 1 H-NMR was measured at room temperature. The content S of the unit obtained from the monomer (a) was calculated using the following formula based on the peak α (4.7 to 5.2 ppm) of the methine structure derived from the vinyl ester unit in the vinyl ester polymer and the peak β (3.6 to 3.8 ppm) of the methyl group derived from the methyl ester part of the unit obtained from the monomer (a).

[0142] S (mol%) = {(number of protons of β / 3) / (number of protons of α+(number of protons of β / 3))}×100

[0143] <Viscosity Measurement of Binder Aqueous Solution and NMP Solution and Calculation of TI>

[0144] The binder aqueous solution with a solid content concentration of 10% by mass and the binder NMP solution with a solid content concentration of 7.5% by mass prepared in each of the examples and comparative examples described below were used as the measurement sample, and the shear rate at 25° C. was measured at 10 s using an E-type viscometer (manufactured by Brucker Field Co., Ltd.). -1 and 100s -1 The viscosity at 25°C with a shear rate of 10 s was calculated from the measured value. -1 The viscosity and shear rate at 100s -1 The viscosity at TI is defined as the viscosity ratio.

[0145] <Evaluation of Stability of Negative Electrode Slurry>

[0146] In order to confirm the stability of the negative electrode slurry prepared in each of the examples and comparative examples described below, the particle sedimentation was visually confirmed immediately after the negative electrode slurry was prepared (after 1 hour). The slurry with no sedimentation was evaluated as ○, and the slurry with sedimentation was evaluated as ×.

[0147] <Determination of Peel Strength (N / m) of Lithium Secondary Batteries in Negative and Positive Electrode Applications>

[0148] For the lithium secondary battery electrodes (negative electrode and positive electrode) prepared in each of the embodiments and comparative examples described below, the strength when the solidified body (derived from the slurry prepared in the embodiments and comparative examples) is peeled off from the copper foil (negative electrode) or aluminum foil (positive electrode) as the current collector is measured. Specifically, the slurry-coated surface of the obtained lithium secondary battery electrode is bonded to a stainless steel plate using a double-sided tape (made by Nichiban Co., Ltd.), and a 50N load cell (made by Imada Co., Ltd.) is used to measure the 180° peel strength (peeling width of 10 mm, peeling speed of 100 mm / min).

[0149] <Determination of Discharge Capacity Retention Rate (%) of Lithium Secondary Batteries in Negative and Positive Electrode Applications>

[0150] The coin cells prepared in the following examples and comparative examples were subjected to rate tests using a commercially available charge and discharge tester (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.). The resistance value when a 0.1 mA current was passed for 3 seconds before initial charging was taken as the DC resistance. During charging, a 0.2 C (approximately 1 mA / cm 2 ) constant current charge, and then 0V constant voltage charge until the current reaches 0.02mA relative to the lithium potential. During discharge, the current is 0.2C (about 0.5mA / cm 2) until 1.5 V. The coin battery was placed in a constant temperature chamber at 25°C, and three cycles of initial charge and discharge were performed under the above conditions. Then, the discharge rate was changed to 2C and one cycle of charge and discharge was performed. The ratio of the 2C discharge capacity to the 0.2C discharge capacity was taken as the discharge capacity retention rate (%).

[0151] <Determination of DC resistance (Ω) of lithium secondary batteries in negative electrode applications>

[0152] The coin cells prepared in the examples and comparative examples described below were tested in the same manner as the above-mentioned discharge capacity retention rate (%) using a commercially available charge and discharge tester (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.) The DC resistance value was evaluated using the resistance value after one charge (fully charged state).

[0153] <Evaluation of NMP Solubility of Positive Electrode Binder Solution>

[0154] In the binder NMP solution for positive electrode application prepared in each of the examples and comparative examples described below, in order to confirm the solubility of NMP, 92.5 parts by mass of NMP was added to 7.5 parts by mass of PVA and stirred, and the temperature was raised to 80°C, and the dissolution of PVA was observed visually. The time from the start of temperature rise to complete dissolution was measured, and the solubility of NMP was evaluated according to the following criteria. The substances evaluated as A or B can be used as binders and have excellent practicality.

[0155] A: Completely dissolved in less than 2 hours.

[0156] B: Complete dissolution in 2 hours or more and less than 4 hours.

[0157] C: Not completely dissolved, and dissolved residues were observed.

[0158] <Evaluation of Uniformity in Positive Electrode Application>

[0159] In order to evaluate the uniformity of the positive electrodes prepared in the examples and comparative examples described below, the state of the positive electrode surface was confirmed by visual inspection. The case where the positive electrode surface was uniform and had no unevenness was judged as ○, and the case where coarse particles were generated due to the aggregation of active materials and the like, resulting in unevenness on the electrode was judged as ×.

[0160] (Manufacturing of PVA)

[0161] [PVA-1]

[0162] 740 parts by mass of vinyl acetate and 260 parts by mass of methanol were added to a reactor equipped with a stirrer, a reflux condenser, a nitrogen inlet, a comonomer addition port, and a polymerization initiator addition port, and the system was purged with nitrogen for 30 minutes while bubbling with nitrogen. Itaconic anhydride was selected as the monomer (a), and the methanol solution of itaconic anhydride (concentration of 20%) was purged with nitrogen by bubbling with nitrogen. The temperature of the reactor was started, and when the internal temperature reached 60°C, 0.25 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added to start polymerization. The methanol solution of itaconic anhydride was added to the above reactor, and after polymerization at 60°C for 3 hours while keeping the monomer composition ratio in the polymerization solution constant, the polymerization was stopped by cooling. The total amount of monomer (a) added until the polymerization was stopped was 2.6 parts by mass, and the solid content concentration at the time of polymerization was stopped was 33.3%. Next, unreacted monomers were removed while adding methanol at any time under reduced pressure at 30°C to obtain a methanol solution of a vinyl ester polymer (concentration of 35%). Next, 9.2 parts by mass of a 10% methanol solution of sodium hydroxide was added to 790.8 parts by mass of a methanol solution of a vinyl ester polymer prepared by further adding methanol to the methanol solution (the polymer in the solution was 200.0 parts by mass), and saponification was performed at 40°C. The concentration of the polymer in the saponified solution was 25%, and the molar ratio of sodium hydroxide to the vinyl acetate unit in the polymer was 0.010. After adding the methanol solution of sodium hydroxide, a gel was generated in about 15 minutes, so it was crushed with a grinder and then placed at 40°C for 1 hour to perform saponification. Thereafter, 500 parts by mass of methyl acetate was added to neutralize the remaining alkali. After confirming the completion of neutralization using a phenolphthalein indicator, a white solid was filtered out. 2000 parts by mass of methanol were added to the white solid, and the mixture was placed at room temperature for 3 hours and washed. This washing operation was repeated three times, and then the liquid was centrifuged and the obtained white solid was heated in a dryer at 120° C. for 4.5 hours to obtain PVA-1. Table 1 summarizes various production materials and properties of PVA-1.

[0163] [PVA-2~PVA-8]

[0164] Various PVAs were produced in the same manner as in the production method of PVA-1, except that polymerization conditions such as the feed amounts of vinyl acetate and methanol, the type and amount of monomer (a) used in polymerization, and the polymerization rate (the reaction rate (%) of the monomers (vinyl acetate and monomer (a)) at the time of stopping the polymerization, calculated by 100×the mass of the vinyl ester polymer at the time of stopping the polymerization / the amount of monomers fed), and saponification conditions such as the molar ratio of sodium hydroxide were changed as shown in Table 1 below. The physical properties of each PVA are summarized in Table 1 below.

[0165] [Table 1]

[0166] .

[0167] Hereinafter, in Examples 1 to 1 to 1-10, the PVA-1 to PVA-7 manufactured above were used to form negative electrodes for lithium secondary batteries, and their performance was evaluated. In Comparative Examples 1-1 to 1-9, the PVA-8 manufactured above and various PVAs described later were used to form negative electrodes for lithium secondary batteries, and their performance was evaluated.

[0168] (Example 1-1)

[0169] Preparation of binder aqueous solution

[0170] In Example 1-1, PVA-1 is used as the PVA used as the binder. First, the modification rate, saponification degree and polymerization degree of PVA-1 are determined by the aforementioned method. Next, water is added to PVA-1, and the mixture is heated and mixed at 80°C for 1 hour to obtain an aqueous binder solution containing a vinyl alcohol polymer and having a solid content concentration of approximately 10% by mass. The solid content concentration is calculated by weighing 3 g of the binder solution into an aluminum cup, and after drying it at 105°C for 3 hours using a hot air dryer, the mass of the remaining solid content is used. For the binder aqueous solution, the viscosity is measured and TI is calculated using the aforementioned method. The physical properties of the binder (modification rate, saponification degree and polymerization degree) and the physical properties of the binder aqueous solution (viscosity and TI) are summarized in Table 2 described below.

[0171] Preparation of negative electrode slurry

[0172] Furthermore, the above-mentioned binder aqueous solution with a solid content concentration of 10% by mass, artificial graphite (FSN-1, manufactured by China Shanshan Company) as a negative electrode active material, and Super-P (manufactured by ティムカル Company) as a conductive aid (conductive imparting agent) are put into a special container, and a planetary mixer (ARE-250, manufactured by Shinki Company) is used for mixing to prepare a negative electrode slurry. When put in, the solid content in the binder aqueous solution is 3 parts by mass, the solid content of artificial graphite is 96 parts by mass, and the solid content of Super-P is 1 part by mass. That is, the composition ratio of the active material, the conductive aid and the binder in the negative electrode slurry is graphite powder: conductive aid: binder = 96:1:3 (mass ratio) in terms of solid content. For the prepared slurry, the stability is evaluated using the above method. The results are summarized in Table 3 described later.

[0173] ·Manufacturing of negative electrode for lithium secondary battery

[0174] The negative electrode slurry obtained as described above was applied to the collector of copper foil (CST8G, Fukuda Metal Foil Powder Industry Co., Ltd.) using a rod coater (T101, made by Matsuo Industry Co., Ltd.). After primary drying with a hot air dryer at 80°C for 30 minutes, rolling treatment was performed using roller pressing (made by Hohsen Co., Ltd.). Thereafter, after punching out as a battery electrode (φ14mm), it took 3 hours at 140°C and secondary drying under reduced pressure conditions to produce a negative electrode for a coin cell. For the produced coin cell negative electrode, the peel strength was measured using the above method. The results are summarized in Table 3 described below.

[0175] Production of lithium secondary batteries

[0176] The negative electrode for the battery obtained as described above was transferred to a glove box (manufactured by Miwa Manufacturing Co., Ltd.) under an argon atmosphere. A metal lithium foil (thickness 0.2 mm, φ16 mm) was used as the positive electrode, and a polypropylene system (セルガード#2400, manufactured by Polypore Co., Ltd.) was used as the separator. For the electrolyte, a mixed solvent system (1M-LiPF6, EC / EMC=3 / 7 vol%, VC2 mass%) obtained by adding vinyl carbonate (VC) to ethylene carbonate (EC) and ethyl methyl carbonate (EMC) was used for lithium hexafluorophosphate (LiPF6) and injected. Coin cells (2032 type) were made using this structure. For the coin cells made, the discharge capacity retention rate and DC resistance value were measured using the above method. The results are summarized in Table 3 described later.

[0177] (Example 1-2)

[0178] Except that PVA-2 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0179] (Example 1-3)

[0180] Except that PVA-3 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, produce the negative electrode for the lithium secondary battery, and produce the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0181] (Examples 1-4)

[0182] Except that PVA-4 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0183] (Examples 1-5)

[0184] Except that PVA-5 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0185] (Examples 1-6)

[0186] Except that PVA-6 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0187] (Example 1-7)

[0188] Except that PVA-7 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0189] (Example 1-8)

[0190] PVA-2 was used as PVA, and a binder NMP solution with a solid content concentration of 7.5% by mass was used instead of a binder aqueous solution. In addition, the same method as in Example 1-1 was used to prepare a negative electrode slurry, a negative electrode for a lithium secondary battery, and a lithium secondary battery, and the same measurements and evaluations were performed. It should be noted that the preparation method of the binder NMP solution with a solid content concentration of 7.5% by mass is the same as the method shown in Example 2-1 described later. The same is true for the following Examples 1-9, Examples 1-10, and Comparative Examples 1-8.

[0191] (Example 1-9)

[0192] PVA-3 was used as PVA, and a binder NMP solution having a solid content concentration of 7.5% by mass was used instead of a binder aqueous solution. In addition, the preparation of the negative electrode slurry, the preparation of the negative electrode for the lithium secondary battery, and the preparation of the lithium secondary battery were carried out by the same method as in Example 1-1, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0193] (Examples 1-10)

[0194] PVA-4 was used as PVA, and a binder NMP solution having a solid content concentration of 7.5% by mass was used instead of a binder aqueous solution. In addition, the preparation of the negative electrode slurry, the preparation of the negative electrode for the lithium secondary battery, and the preparation of the lithium secondary battery were carried out by the same method as in Example 1-1, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0195] (Comparative Example 1-1)

[0196] As PVA, PVA with a polymerization degree of 1700, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 1-1 was used to prepare the binder aqueous solution, prepare the negative electrode slurry, prepare the negative electrode for the lithium secondary battery, and prepare the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0197] (Comparative Example 1-2)

[0198] As PVA, PVA with a polymerization degree of 2400, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 1-1 was used to prepare the binder aqueous solution, prepare the negative electrode slurry, prepare the negative electrode for the lithium secondary battery, and prepare the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0199] (Comparative Examples 1-3)

[0200] As PVA, a PVA having a polymerization degree of 3500, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 1-1 was used to prepare the binder aqueous solution, prepare the negative electrode slurry, prepare the negative electrode for the lithium secondary battery, and prepare the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0201] (Comparative Examples 1-4)

[0202] As PVA, a PVA having a polymerization degree of 4500, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 1-1 was used to prepare the binder aqueous solution, prepare the negative electrode slurry, prepare the negative electrode for the lithium secondary battery, and prepare the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0203] (Comparative Examples 1-5)

[0204] As PVA, a PVA having a polymerization degree of 4500, a modification rate of 0, and a saponification degree of 95 was used. In addition, the same method as in Example 1-1 was used to prepare the binder aqueous solution, prepare the negative electrode slurry, prepare the negative electrode for the lithium secondary battery, and prepare the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0205] (Comparative Examples 1-6)

[0206] Except that PVA-8 was used as PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, prepare the negative electrode slurry, make the negative electrode for the lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0207] (Comparative Examples 1-7)

[0208] Except that polyacrylic acid (molecular weight 250,000, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of PVA, the same methods as in Example 1-1 were used to prepare the binder aqueous solution, the negative electrode slurry, the negative electrode for the lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0209] (Comparative Examples 1-8)

[0210] As PVA, a PVA with a polymerization degree of 3500, a modification rate of 0, and a saponification degree of 88 was used, and a binder NMP solution with a solid content concentration of 7.5% by mass was used instead of a binder aqueous solution. In addition, the preparation of the negative electrode slurry, the preparation of the negative electrode for the lithium secondary battery, and the preparation of the lithium secondary battery were carried out by the same method as in Example 1-1, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described later.

[0211] (Comparative Examples 1-9)

[0212] As a negative electrode binder composition, a 10 mass % aqueous solution of a water-soluble lithium-modified isobutylene-maleic anhydride copolymer resin (average molecular weight 470,000, degree of neutralization 1.0, ring opening rate 100%) was prepared. The lithium-modified isobutylene-maleic anhydride copolymer resin was prepared by adding 2 equivalents of lithium hydroxide to the maleic anhydride unit in the isobutylene-maleic anhydride copolymer.

[0213] Except that the above binder composition was used instead of PVA, the negative electrode slurry was prepared, the negative electrode for lithium secondary battery was produced, and the lithium secondary battery was produced in the same manner as in Example 1-1, and the same measurements and evaluations were performed. The results are summarized in Tables 2 and 3 described below.

[0214] [Table 2]

[0215] .

[0216] [Table 3]

[0217] .

[0218] As shown in Table 3, the slurry of the Example was stable, had good peel strength, high discharge capacity retention rate, and low DC resistance value compared to the Comparative Example, which means that the electrode was uniformly formed.

[0219] Hereinafter, in Examples 2-1 to 2-7, the PVA-1 to PVA-7 manufactured above were used to form a positive electrode for a lithium secondary battery, and their performance was evaluated. In Comparative Examples 2-1 to 2-8, the PVA-8 manufactured above and various PVAs described later were used to form a negative electrode for a lithium secondary battery, and their performance was evaluated.

[0220] (Example 2-1)

[0221] Preparation of binder NMP solution

[0222] In Example 2-1, PVA-1 is used as the PVA used as the binder. 92.5 parts by mass of NMP (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) are added to 7.5 parts by mass of PVA-1, and the temperature is raised to 80°C while stirring. Furthermore, the mixture is heated and stirred until it is visually confirmed to be completely dissolved, thereby obtaining a binder NMP solution containing a vinyl alcohol polymer and having a solid content concentration of about 7.5% by mass. The solid content concentration is calculated by weighing 3 g of the binder solution into an aluminum cup and drying it at 120°C for 4 hours using a hot air dryer, and then calculating the mass of the remaining solid content. For the binder NMP solution, the viscosity is measured and TI is calculated using the aforementioned method. Furthermore, for the prepared binder NMP solution, the solubility of NMP is evaluated using the aforementioned method. The evaluation results of the physical properties (modification rate, saponification degree and polymerization degree) of the binder, the physical properties (viscosity and TI) of the binder NMP solution and the solubility of NMP are summarized in Table 4 described later.

[0223] Preparation of positive electrode slurry

[0224] Furthermore, the binder NMP solution with a solid content concentration of about 7.5% by mass, NCM (manufactured by Nippon Chemical Industry Co., Ltd., "Celsil C-5H") as a positive electrode active material, and Super-P (manufactured by TIMUKARU Co., Ltd.) as a conductive aid (conductive imparting agent) are put into a dedicated container, and a planetary mixer (ARE-250, manufactured by Shinki Co., Ltd.) is used for kneading to prepare a positive electrode slurry. When put in, the solid content in the binder NMP solution is 3 parts by mass, the NCM is 95 parts by mass, and the solid content of Super-P is 2 parts by mass. That is, the composition ratio of the active material, the conductive aid, and the binder in the positive electrode slurry is NCM powder: conductive aid: binder = 95:2:3 (mass ratio) in terms of solid content.

[0225] ·Production of positive electrode for lithium secondary battery

[0226] The positive electrode slurry obtained as described above was applied to the collector of aluminum foil (CST8G, Fukuda Metal Foil Powder Industry Co., Ltd.) using a rod coater (T101, made by Matsuo Industry Co., Ltd.). After primary drying with a hot air dryer at 80°C for 30 minutes, the calendering treatment was performed using a roller press (made by Hohsen Co., Ltd.). Thereafter, after punching out as a battery electrode (φ14mm), it took 3 hours at 140°C and was dried twice under reduced pressure to produce a positive electrode for a coin cell. For the produced coin cell positive electrode, the peel strength was measured and the uniformity of the positive electrode was evaluated using the aforementioned method. The results are summarized in Table 5 described below.

[0227] Production of lithium secondary batteries

[0228] The positive electrode for the battery obtained as described above was transferred to a glove box (manufactured by Miwa Manufacturing Co., Ltd.) under an argon atmosphere. A metal lithium foil (thickness 0.2 mm, φ16 mm) was used as the negative electrode, and a polypropylene system (セルガード#2400, manufactured by Polypore) was used as the separator. For the electrolyte, a mixed solvent system (1M-LiPF6, EC / EMC=3 / 7 vol%, VC2 mass%) obtained by adding vinyl carbonate (VC) to ethylene carbonate (EC) and ethyl methyl carbonate (EMC) was used for lithium hexafluorophosphate (LiPF6) and injected. Coin cells (2032 type) were made using this structure. For the coin cells made, the discharge capacity retention rate was measured using the above method. The results are summarized in Table 5 described later.

[0229] (Example 2-2)

[0230] PVA-2 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, prepare the positive electrode slurry, make the positive electrode for lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0231] (Example 2-3)

[0232] PVA-3 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, the positive electrode slurry, the positive electrode for lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0233] (Example 2-4)

[0234] As PVA, PVA-4 was used. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, prepare the positive electrode slurry, make the positive electrode for lithium secondary battery, and make the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0235] (Example 2-5)

[0236] PVA-5 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, the positive electrode slurry, the positive electrode for lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0237] (Example 2-6)

[0238] PVA-6 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, the positive electrode slurry, the positive electrode for lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0239] (Example 2-7)

[0240] PVA-7 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, the positive electrode slurry, the positive electrode for lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0241] (Comparative Example 2-1)

[0242] As PVA, a PVA having a polymerization degree of 1700, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 2-1 was used to prepare a binder NMP solution, prepare a positive electrode slurry, prepare a positive electrode for a lithium secondary battery, and prepare a lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0243] (Comparative Example 2-2)

[0244] As PVA, a PVA having a polymerization degree of 2400, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 2-1 was used to prepare a binder NMP solution, prepare a positive electrode slurry, prepare a positive electrode for a lithium secondary battery, and prepare a lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0245] (Comparative Example 2-3)

[0246] As PVA, a PVA having a polymerization degree of 3500, a modification rate of 0, and a saponification degree of 88 was used. In addition, the same method as in Example 2-1 was used to prepare a binder NMP solution, prepare a positive electrode slurry, prepare a positive electrode for a lithium secondary battery, and prepare a lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0247] (Comparative Example 2-4)

[0248] As PVA, a PVA having a polymerization degree of 4500, a modification rate of 0, and a saponification degree of 88 was used. In addition, the binder NMP solution was prepared by the same method as in Example 2-1. However, it was not completely dissolved in the binder NMP solution, so it was impossible to prepare the positive electrode slurry, make the positive electrode for the lithium secondary battery, and make the lithium secondary battery. The results that can be measured are summarized in Table 4 described later.

[0249] (Comparative Example 2-5)

[0250] As PVA, a PVA having a polymerization degree of 4500, a modification rate of 0, and a saponification degree of 95 was used. In addition, the binder NMP solution was prepared by the same method as in Example 2-1. However, it was not completely dissolved in the binder NMP solution, so it was impossible to prepare the positive electrode slurry, make the positive electrode for the lithium secondary battery, and make the lithium secondary battery. The results that can be measured are summarized in Table 4 described later.

[0251] (Comparative Example 2-6)

[0252] PVA-8 was used as PVA. In addition, the same method as in Example 2-1 was used to prepare the binder NMP solution, the positive electrode slurry, the positive electrode for lithium secondary battery, and the lithium secondary battery, and the same measurements and evaluations were performed. The results are summarized in Tables 4 and 5 described later.

[0253] (Comparative Example 2-7)

[0254] Instead of PVA, polyacrylic acid (molecular weight 250,000, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. In addition, the binder NMP solution was prepared by the same method as in Example 2-1. However, it was not completely dissolved in the binder NMP solution, so it was impossible to prepare the positive electrode slurry, make the positive electrode for the lithium secondary battery, and make the lithium secondary battery. The results that can be measured are summarized in Table 4 described later.

[0255] (Comparative Example 2-8)

[0256] A 10% aqueous solution of a water-soluble lithium-modified isobutylene-maleic anhydride copolymer resin (average molecular weight of 470,000, degree of neutralization of 1.0, and ring opening rate of 100%) was prepared. The lithium-modified isobutylene-maleic anhydride copolymer resin was prepared by adding 2 equivalents of lithium hydroxide to the maleic anhydride unit in the isobutylene-maleic anhydride copolymer. The 10% aqueous solution was dried at 120°C, and the binder NMP solution was prepared for the obtained solid using the same method as in Example 2-1. However, it was not completely dissolved in the binder NMP solution, so it was impossible to prepare the positive electrode slurry, make the positive electrode for the lithium secondary battery, and make the lithium secondary battery. The results that can be measured are summarized in Table 4 described later.

[0257] [Table 4]

[0258] .

[0259] [Table 5]

[0260] .

[0261] As shown in Table 5, the Examples formed uniform electrodes, had extremely excellent peel strength, and had a high discharge capacity retention rate, compared with the Comparative Examples.

[0262] The binder of the present invention can form a uniform electrode even for an active material used in a lithium primary battery and can exhibit excellent peel strength. In Reference Examples 1-1 and 1-2, a positive electrode for a lithium primary battery was formed from the PVA-2 or PVA-4 produced above, and its performance was evaluated.

[0263] (Reference Example 1-1)

[0264] PVA-2 was used, and the aforementioned binder aqueous solution with a solid content concentration of 10% by mass and electrolytic manganese dioxide as the positive electrode active material were used. In addition, the same method as in Example 2-1 was used to prepare the positive electrode slurry, produce the positive electrode for the lithium primary battery, and produce the lithium primary battery. The electrode uniformity and peel strength were measured and evaluated in the same manner. The results are shown in Table 6 described below.

[0265] (Reference Example 1-2)

[0266] Except that PVA-4 was used instead of PVA-2, the same method as Reference Example 1-2 was used to prepare the positive electrode slurry, produce the positive electrode for lithium primary battery, and produce the lithium primary battery, and the same measurement and evaluation were performed on the electrode uniformity and peel strength. The results are shown in Table 6 described below.

[0267] [Table 6]

[0268] 。

Claims

1. A non-aqueous electrolyte battery electrode binder comprising a water-soluble resin, The water-soluble resin is a vinyl alcohol polymer comprising a vinyl alcohol unit and a unit derived from the monomer (a), The monomer (a) is at least one selected from the group consisting of a carboxylic acid having an unsaturated double bond, an alkyl ester of the carboxylic acid, an anhydride of the carboxylic acid, and a salt of the carboxylic acid. The non-aqueous electrolyte battery electrode binder is in an aqueous solution state with a solid content concentration of 10% by mass, and the shear rate of the aqueous solution at 25° C. is 10 s -1 The viscosity of the aqueous solution is 4 Pa·s or more and 30 Pa·s or less, and the shear rate of the aqueous solution at 25° C. is 10 s -1 The viscosity and shear rate at 100s -1 The thixotropic index defined by the viscosity ratio when the viscosity is 1.8 or more and 5 or less.

2. The non-aqueous electrolyte battery electrode binder according to claim 1, wherein In the state of N-methyl-2-pyrrolidone solution with a solid content concentration of 7.5 mass %, the shear rate of the solution at 25° C. is 10 s -1 The viscosity of the solution is 4 Pa·s or more and 35 Pa·s or less, and the shear rate of the solution at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity at which the thixotropic index is defined as the viscosity ratio is 2 or more and 6 or less.

3. The non-aqueous electrolyte battery electrode binder according to claim 1 or 2, wherein: The water-soluble resin is a vinyl alcohol polymer having a cross-linked structure.

4. The non-aqueous electrolyte battery electrode binder according to claim 1 or 2, wherein The modification rate of the water-soluble resin is 0.02 mol% or more and 5 mol% or less based on the number of moles of all monomer units constituting the water-soluble resin.

5. A non-aqueous electrolyte battery electrode binder solution comprising the non-aqueous electrolyte battery electrode binder according to any one of claims 1 to 4 and water, The shear rate of the non-aqueous electrolyte battery electrode binder solution at 25° C. is 10 s -1 The viscosity is 4 Pa·s or more and 30 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The thixotropic index defined by the viscosity ratio when the viscosity is 1.8 or more and 5 or less.

6. A non-aqueous electrolyte battery electrode binder solution comprising the non-aqueous electrolyte battery electrode binder according to any one of claims 1 to 4 and N-methyl-2-pyrrolidone, The shear rate of the non-aqueous electrolyte battery electrode binder solution at 25° C. is 10 s -1 The viscosity is 4 Pa·s or more and 35 Pa·s or less, and the shear rate at 25°C is 10 s -1 The viscosity and shear rate at 100s -1 The viscosity at which the thixotropic index is defined as the viscosity ratio is 2 or more and 6 or less. 7 . A non-aqueous electrolyte battery electrode slurry comprising the non-aqueous electrolyte battery electrode binder solution according to claim 5 or 6 and an active material.

8. The non-aqueous electrolyte battery electrode slurry according to claim 7, wherein The content of the nonaqueous electrolyte battery electrode binder is 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the active material. 9 . A non-aqueous electrolyte battery electrode comprising a solidified body of the non-aqueous electrolyte battery electrode slurry according to claim 7 or 8 and a current collector. 10 . A non-aqueous electrolyte battery comprising the non-aqueous electrolyte battery electrode according to claim 9 .

Citation Information

Patent Citations

  • Binder containing vinyl alcohol polymer, slurry, nonaqueous electrolyte secondary battery, and its electrode

    JP1999250915A

  • Method for manufacturing positive electrode plate

    JP2013037955A

  • Binder composition for secondary battery electrode, secondary battery electrode, and secondary battery

    JP2017059527A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, and method for producing the same, and nonaqueous electrolyte secondary battery

    JP2017107827A

  • Process for producing multilayer film

    CN104321149A