Method for manufacturing electrode binder and electrode assembly containing the electrode binder

Through the dissolution of granulated polyvinylidene fluoride in the solvent and the addition of conductive materials, the problems of poor solubility and insufficient adhesion of the secondary battery electrode adhesive are solved, and efficient dispersion of active materials and improved battery performance are achieved.

CN113728472BActive Publication Date: 2024-11-22LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080030296.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-15
Filing Date
2020-07-03
Publication Date
2024-11-22
Estimated Expiration
2040-07-03

AI Technical Summary

Technical Problem

The existing secondary battery electrode adhesives have poor solubility in the solvent, which leads to difficulty in uniform dispersion of active materials and insufficient adhesion, which affects the safety and performance of the battery.

Method used

By dissolving the particle size in the solvent by granulated polyvinylidene fluoride (PVDF), the particle diameter is controlled within the range of 0.5 to 5 mm, and conductive material is added to form an electrode composite layer with high porosity and uniform dispersion, thereby improving adhesion.

Benefits of technology

The dispersion and adhesion of the electrode composite are significantly improved, the impurity content is reduced, and the safety and performance stability of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113728472B_ABST
    Figure CN113728472B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing an electrode binder and an electrode assembly comprising the electrode binder, the method comprising the step of dissolving granulated polyvinylidene fluoride (PVDF) in a solvent. The present invention can provide an electrode assembly having a low content of impurities in a binder solution, being able to improve the dispersion of an electrode active material, and exhibiting excellent bonding force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an electrode binder and an electrode composite comprising the binder prepared by the method.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0085287, filed on Jul. 15, 2019, and the entire contents of the Korean Patent Application are incorporated herein by reference. Background Art

[0003] With the increase in technological development and demand for mobile devices, the demand for secondary batteries is also increasing sharply. Among them, lithium secondary batteries are widely used as energy sources for various electronic products and various mobile devices due to their high energy density and high operating voltage as well as excellent storage and life characteristics. In addition, secondary batteries have attracted attention as energy sources for electric vehicles, hybrid electric vehicles, etc., which have been proposed as solutions to air pollution of existing gasoline vehicles and diesel vehicles using fossil fuels. Therefore, the types of applications currently using secondary batteries are very diverse due to the advantages of secondary batteries, and it is expected that secondary batteries will be used in many fields and products in the future.

[0004] As the application fields and products of secondary batteries are diversified as described above, the types of batteries are also diversified to provide suitable output and capacity. In addition, miniaturization or lightness is strongly required for batteries applied to the above fields and products.

[0005] The secondary battery includes a structure in which a separator is interposed between two electrodes including a positive electrode and a negative electrode. The electrode has a structure in which a composite layer in which an active material is dispersed in a binder matrix is ​​coated on an electrode current collector.

[0006] In order to simultaneously achieve the high output and miniaturization required of secondary batteries, a technology is needed to uniformly disperse the active material on the electrode current collector while making the battery thinner. In addition, it is also necessary to improve the adhesion of the binder to improve the safety of the secondary battery. Summary of the invention

[0007] [Technical issues]

[0008] The present invention has been accomplished in order to solve the above-mentioned problems, and an object of the present invention is to provide a method for manufacturing an electrode binder containing polyvinylidene fluoride (PVDF) and an electrode composite including the same.

[0009] [Technical solution]

[0010] The method of manufacturing an electrode binder according to the present invention includes the step of dissolving particle-formed polyvinylidene fluoride (PVDF) in a solvent.

[0011] According to one embodiment of the present invention, the granulated polyvinylidene fluoride (PVDF) may be in a form in which powdery particles are aggregated to be granulated, and an average diameter of the particles may be in the range of 0.5 to 5 mm.

[0012] According to one embodiment of the present invention, the length ratio of the major axis to the minor axis of the PVDF particles may be in the range of 20:1 to 1:1.

[0013] According to one embodiment of the present invention, the powdery particles may include one or more of the following: a weight average molecular weight (Mw) of 2.0×10 5 ~7.5×10 5 The first powder particles; and a weight average molecular weight (Mw) of 7.5×10 5 ~2.5×10 6 of second powder particles.

[0014] According to one embodiment of the present invention, the solvent may be a water-soluble solvent having a polar group.

[0015] Specifically, the solvent may be at least one selected from the group consisting of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, and water.

[0016] According to one embodiment of the present invention, the content of polyvinylidene fluoride dissolved in the solvent may be in the range of 1% to 25% (weight / weight).

[0017] According to one embodiment of the present invention, the present invention may further include a step of adding a conductive material during or after the step of dissolving the granulated polyvinylidene fluoride (PVDF) in a solvent.

[0018] The present invention may also provide an electrode composite comprising the electrode binder.

[0019] According to one embodiment of the present invention, the electrode composite of the present invention comprises: an electrode current collector; and an electrode composite layer coated on one or both surfaces of the electrode current collector, the electrode composite layer comprising: a particulate active material; a binder comprising polyvinylidene fluoride (PVDF); and a conductive material, wherein:

[0020] The electrode composite layer is filled with a particulate active material, and the gaps between the active material particles are filled with a binder and a conductive material, the gaps have a porosity of 15% to 35% (volume / volume), and an average diameter of the gaps is 0.01 to 1 mm.

[0021] According to one embodiment of the present invention, based on the cross-section of the electrode composite layer, the particulate active material may include: first particles having an average particle size in the range of 5 to 10 μm; and second particles having an average particle size in the range of 100 to 200 μm, and the ratio of the areas occupied by the first particles and the second particles may be in the range of 1:1 to 10:1.

[0022] According to one embodiment of the present invention, the coating film of the electrode composite layer may have an average thickness of 50 to 150 μm, and for a sample 2 cm wide and 20 cm long, the adhesion between the electrode collector layer and the composite layer mixed with active material, conductive material and binder may be 100 N / m or more.

[0023] Beneficial Effects

[0024] The method for manufacturing an electrode binder according to the present invention can provide an electrode composite having a low impurity content in a solution, a high dispersion of an electrode active material, a binder, and a conductive material, and excellent adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a photograph of a binder solution after filtering the binder solution in which the stirring process according to one embodiment of the present invention has been completed through a 200-mesh filter.

[0026] Figure 2 is a photograph of a binder solution after filtering the binder solution in which the stirring process according to a comparative example of the present invention has been completed through a 200-mesh filter.

[0027] Figure 3 and 4 Observation results of a cross section of an electrode composite according to one embodiment of the present invention are shown.

[0028] Figure 5 and 6 Observation results of a cross section of an electrode composite according to a comparative example are shown. DETAILED DESCRIPTION

[0029] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms and words used in this specification and claims should not be interpreted as limited to common or dictionary terms, and the inventor may appropriately define the concepts of the terms to best describe his invention. The terms and words should be interpreted as meanings and concepts consistent with the technical ideas of the present invention.

[0030] The present invention provides a polyvinylidene fluoride (PVDF)-based electrode binder and a method for manufacturing the same. Specifically, the electrode binder according to the present invention is prepared by dissolving granulated polyvinylidene fluoride in a solvent.

[0031] Polyvinylidene fluoride is used as an electrode binder for secondary batteries, but the problem is that the solubility in the solvent is poor. The reduced solubility in the solvent increases the impurity content of the binder component, and becomes the reason for suppressing the uniform dispersion of the active material when mixed with the active material. Specifically, the polyvinylidene fluoride in powder form has a problem of slow dissolution rate due to its small bulk density and poor solvent wettability. In addition, the added polyvinylidene fluoride floats in a large amount on the upper layer of the solvent and hardly receives the shear stress applied to the solvent during stirring.

[0032] In the present invention, powdered polyvinylidene fluoride is granulated and dissolved in a solvent, thereby improving solubility and dispersibility in the solvent. The granulated polyvinylidene fluoride is in a form in which powdered particles are agglomerated and granulated. The average diameter of the particles can be controlled within the range of 0.5 to 5 mm. Specifically, the average diameter of the particles is within the range of 0.5 to 4 mm, 0.5 to 2.5 mm, 1 to 3.5 mm, 2 to 4.5 mm, 3.5 to 5 mm or 1 to 3 mm. By controlling the average diameter of the particles within the above range, sufficient packing density is provided and the formation of floating objects is prevented. When the average diameter of the particles is too large, the surface area per unit weight is reduced, so that the solubility may be reduced.

[0033] In another example, the present invention includes a case where two or more particle groups having different average particle sizes are mixed and used. For example, the particles may include: a first particle group having an average diameter of 0.5 to 2.5 mm; and a second particle group having an average diameter in the range of 3.5 to 5 mm. The first particle group and the second particle group may be used in a mixing ratio of 1:1 to 10:1. By mixing and using particle groups having different particle sizes, there is an effect of improving dispersibility and solubility and reducing the generation of bubbles when preparing an adhesive.

[0034] In one embodiment, the shape of the particles is a cylinder, a cuboid, or a sphere with an elliptical cross section. In addition, the particles are in a form in which the length ratio of the major axis to the minor axis is in the range of 20:1 to 1:1. Specifically, the length ratio of the major axis to the minor axis of the particles is in the range of 17:1 to 3:1, 15:1 to 5:1, or 13:1 to 7:1. By forming the particles in a form extending in one direction, the surface area per unit weight can be increased while ensuring the packing density.

[0035] The particles are in the form of agglomerated powdered particles. The powdered particles may be controlled within a range that provides a sufficient surface area while forming the particles. For example, the powdered particles may include one or more of the following: a weight average molecular weight (Mw) of 2.0×105 ~7.5×10 5 The first powder particles; and a weight average molecular weight (Mw) of 7.5×10 5 ~2.5×10 6 The first or second powder particles or a mixture of the two particles can be used as the powdery particles. More specifically, the weight average molecular weight of the first powder particles is between 2.5×10 5 ~7.0×10 5 , 3.0×10 5 ~6.5×10 5 or 3.5 × 10 5 ~6.0×10 5 In addition, the weight average molecular weight of the second powder particles is more specifically within the range of 1.0×10 6 ~2.2×10 6 , 1.2×10 6 ~2.0×10 6 or 1.4×10 6 ~1.8×10 6 The inventors of the present invention have confirmed through various repeated experiments that by controlling the weight average molecular weight of the powdery particles within the above range, the formulation stability of the particles can be improved without impairing the wettability to the solvent.

[0036] In one example, the present invention agglomerates powdered particles to form particles. In this case, powder particles having different weight average molecular weights can be used, but particles having different particle sizes can be formed for various powder particles. For example, the second particle group can be formed by using the first powder particles, and the first particle group can be formed by using the second powder particles. Thus, the packing density of the prepared particles can be maintained and the solubility in the solvent can be increased. In another example, the first particle group can also be formed by using the first powder particles, and the second particle group can be formed by using the second powder particles.

[0037] The present invention provides a method for preparing a polyvinylidene fluoride-based adhesive. Examples of polyvinylidene fluoride include one or more of the following: polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polyvinylidene fluoride-co-tetrafluoroethylene, polyvinylidene fluoride-co-trifluoroethylene, polyvinylidene fluoride-co-chlorotrifluoroethylene, and polyvinylidene fluoride-co-ethylene.

[0038] The polyvinylidene fluoride adhesive may be used alone or in combination with an acrylic adhesive. In the case of such a combination, advantageous characteristics of the acrylic adhesive may be utilized depending on the combination ratio.

[0039] The acrylic adhesive may be a copolymer including: at least one first functional group selected from the group consisting of an -OH group and a -COOH group; and at least one second functional group selected from the group consisting of an amine group and an amide group.

[0040] Specifically, the acrylic binder may have a repeating unit derived from a monomer having a first functional group and a repeating unit derived from a monomer having a second functional group. Such an acrylic binder together with a polyvinylidene fluoride-based binder can form a uniform electrode composite layer on the electrode, prevent layer separation, and provide electrochemical performance and stability.

[0041] The solvent used in the present invention can be used without limitation, as long as polyvinylidene fluoride can be fully dissolved. Specifically, the solvent is a water-soluble solvent having a polar group.

[0042] The non-limiting examples of the solvent include acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water or a mixture thereof. Specifically, the solvent can be N-methyl-2-pyrrolidone (NMP). Such solvents have excellent polyvinylidene fluoride solubility and provide an appropriate level of viscosity, so that a slurry coating can be formed on the surface of an electrode collector at a desired level.

[0043] An appropriate amount of granulated polyvinylidene fluoride is added to the solvent. Specifically, the content of polyvinylidene fluoride dissolved in the solvent is in the range of 1% to 25% (weight / weight). By controlling the content of polyvinylidene fluoride within the above range, a suitable viscosity level can be achieved and the occurrence of suspended matter can be minimized.

[0044] In one embodiment, the present invention further comprises a step of adding a conductive material during or after the step of dissolving the granulated polyvinylidene fluoride (PVDF) in a solvent. There is no particular limitation on this conductive material as long as it has high conductivity and does not cause chemical changes in the battery, and examples thereof include: graphite such as natural graphite and artificial graphite; carbon black-like substances such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; fluorocarbons; metal powders such as aluminum and nickel powders; conductive whiskers such as zinc oxide and potassium titanate; conductive oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives, etc.

[0045] The present invention also provides an electrode composite comprising the binder prepared by the above method. In the present specification, the term "electrode composite" is understood to mean a structure in which a composite layer of an active material, a binder and a conductive material is formed on an electrode current collector.

[0046] The electrode composite of the present invention comprises: an electrode current collector; and an electrode composite layer coated on one or both surfaces of the electrode current collector. Here, the electrode composite layer comprises: a particulate active material; and polyvinylidene fluoride (PVDF) and a conductive material. In one embodiment, the electrode composite layer is filled with the particulate active material, and the gaps between the active material particles are filled with a binder and a conductive material.

[0047] The porosity of the voids is 15% to 35% (volume / volume), and the average diameter of the voids is 0.01 to 1 mm. More specifically, the porosity is 20% to 30% (volume / volume), and the average diameter of the voids is 0.1 to 0.5 mm. In the present invention, by controlling the porosity of the voids and the average diameter of the voids as described above, the particulate active material, binder and conductive material can be uniformly dispersed in the electrode composite layer.

[0048] Based on the cross section of the electrode composite layer, the particulate active material may include particles with different particle sizes. Specifically, the particulate active material may include: first particles with an average particle size of 5 to 10 μm; and second particles with an average particle size of 100 to 200 μm. In the present invention, the situation where a particulate active material with a uniform particle size is dispersed in the electrode composite layer is not excluded. However, by mixing the first and second particles with different particle sizes, the porosity in the electrode composite layer can be reduced and the dispersion density of the active material can be increased. In addition, when the first particle and the second particle are mixed, the ratio of the area occupied by the first particle and the second particle can be controlled within the range of 1:1 to 10:1. This is the ratio of the area occupied by each particle based on the cross section of the electrode composite layer.

[0049] In addition, the electrode composite according to the present invention provides excellent adhesion between the electrode collector layer and the electrode composite layer. For example, under the condition that the coating thickness of the electrode composite layer is 50 to 150 μm, the adhesion between the electrode collector layer and the electrode composite layer is 100 N / m or more. Specifically, the adhesion is in the range of 110 to 150 N / m or 115 to 125 N / m.

[0050] In one embodiment, the electrode active materials (i.e., positive electrode active materials and negative electrode active materials) and electrode current collectors (i.e., positive electrode current collectors and negative electrode current collectors) of the present invention are not particularly limited and can be prepared according to conventional methods known in the art or modified methods thereof.

[0051] The positive electrode active material may include a compound using a lithium intercalation material as its main component: for example, a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2) or a compound substituted by one or more transition metals; a lithium manganese oxide such as Li 1+x Mn 2-x O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3 and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiFe3O4, V2O5 and Cu2V2O7; 1-x M x Lithium nickel oxide represented by LiMn O2 (herein, M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x = 0.01 to 0.3); 2-x M x Lithium manganese composite oxides represented by Li2Mn3MO8 (herein, M=Co, Ni, Fe, Cr, Zn or Ta, and x=0.01~0.1) or Li2Mn3MO8 (herein, M=Fe, Co, Ni, Cu or Zn); LiMn2O4 in which part of the Li in the formula is replaced by alkaline earth metal ions; disulfide compounds; and Fe2(MoO4)3 or composite oxides formed by combinations thereof, but not limited thereto.

[0052] The positive electrode current collector may have a thickness of 3 to 500 μm. There is no particular limitation on the positive electrode current collector as long as it has conductivity and does not cause chemical changes in the battery. Examples of the positive electrode current collector include: stainless steel, aluminum, nickel, titanium, sintered carbon; or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc. The electrode current collector may have fine concavoconvexities on its surface to improve the adhesion of the positive electrode composite, and various forms such as films, sheets, foils, meshes, porous bodies, foams and non-woven fabrics are all possible.

[0053] The binder is a component that helps to bind the positive electrode active material particles to the conductive material and to the electrode current collector. For example, based on the total weight of the mixture containing the positive electrode active material, the binder is added in an amount of 1 to 50% by weight. Because this binder is the same as described above, its detailed description will be omitted here. The binder may also contain a conductive material. The conductive material may be pre-mixed with the binder, or may be mixed with the positive electrode active material. Based on the total weight of the mixture containing the positive electrode active material, the amount of such conductive material added may be, for example, 1 to 50% by weight.

[0054] In addition, the negative electrode is manufactured by coating negative electrode active material particles on a negative electrode current collector and drying the negative electrode, and may further contain components such as the above-mentioned conductive material, a binder, and a solvent as needed.

[0055] The thickness of the negative electrode current collector can be 3 to 500 μm. There is no particular limitation on the negative electrode current collector as long as it has electrical conductivity and does not cause chemical changes in the battery. Examples thereof include: copper, stainless steel, aluminum, nickel, titanium, sintered carbon; copper or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc.; aluminum-cadmium alloy, etc. In addition, like the positive electrode current collector, fine irregularities can be formed on the surface to enhance the bonding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabrics.

[0056] Examples of the negative electrode active material include: carbon such as non-graphitized carbon and graphitic carbon; metal composite oxides such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups 1, 2, and 3 in the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium alloys; silicon alloys; tin alloys; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; and Li-Co-Ni-based materials.

[0057] The electrode composite of the present invention can be manufactured, for example, as follows.

[0058] First, the electrode composite layer is coated on one or both surfaces of the electrode current collector. The electrode current collector and the electrode composite layer are as described above regarding the structure of the electrode composite.

[0059] A binder solution is generated by dissolving a binder for a desired electrode active material (e.g., a positive electrode active material or a negative electrode active material) in a solvent, and then the desired electrode active material particles are added to the generated binder solution. In this mixture, the electrode active material particles are uniformly dispersed in the binder solution by a method such as stirring, thereby preparing an active material slurry. The prepared active material slurry is applied to one or both surfaces of the electrode current collector in the form of a layer.

[0060] The active material slurry can be applied using conventional coating methods known in the art such as dip coating, die coating, roller coating, comma coating or a mixture thereof. One of the various methods described above can be used to continuously or discontinuously. In particular, from the perspective of productivity, it is preferred that multiple electrode current collectors are coated continuously or simultaneously.

[0061] The solvent is removed from the active material slurry applied on the electrode current collector. For example, the solvent can be removed by a drying process. The active material slurry applied on the electrode current collector is dried simultaneously or separately to remove the solvent, thereby obtaining an electrode assembly.

[0062] When the active material slurry is applied by coating, a solvent may be added to the coating solution. In this case, an additional drying process is required for the coating. The drying conditions may be batch or continuous using an oven or a heating chamber within a temperature range taking into account the vapor pressure of the solvent used.

[0063] In addition, the electrode composite of the present invention can be used as an electrode composite of an electrochemical device. Such electrochemical devices include all devices that undergo electrochemical reactions, and specific examples include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors such as supercapacitor devices. In particular, among secondary batteries, lithium secondary batteries including lithium metal secondary batteries, lithium ion secondary batteries, lithium polymer secondary batteries, or lithium ion polymer secondary batteries are preferred.

[0064] The electrochemical device can be manufactured according to conventional methods well known in the art. For example, the above electrode composite, ie, the positive electrode and the negative electrode, can be assembled by inserting a conventional separator in the art, and then injecting an electrolyte to manufacture the electrochemical device.

[0065] The separator used with the electrode composite according to one embodiment of the present invention is not particularly limited and may be prepared in a porous form combined with inorganic / organic particles or the like according to a conventional method known in the art.

[0066] Furthermore, heterogeneous electrodes or electrode composites manufactured according to the manufacturing method of the present invention, ie, a positive electrode composite and a negative electrode composite, are respectively arranged so that their porous binder layers face each other with a separator disposed therebetween to be wound or laminated, thereby manufacturing an electrochemical device.

[0067] Specifically, an electrochemical device may be provided, the electrochemical device comprising a positive electrode composite having a porous adhesive layer on one surface, a negative electrode composite having a porous adhesive layer on one surface, and a separator disposed between the porous adhesive layer of the positive electrode composite and the porous adhesive layer of the negative electrode composite. In another embodiment, the electrochemical device is characterized in that it is a lithium secondary battery.

[0068] Furthermore, the injection of the electrolyte can be performed at an appropriate step in the battery manufacturing process, depending on the manufacturing process and the desired physical properties of the final product. That is, it can be applied before battery assembly or at the final stage of battery assembly.

[0069] In addition, the electrochemical device of the present invention includes all devices that undergo electrochemical reactions, and specific examples can be all types of primary batteries, secondary batteries, fuel cells, solar cells or capacitors such as supercapacitor devices. In particular, among secondary batteries, lithium secondary batteries including lithium metal secondary batteries, lithium ion secondary batteries, lithium polymer secondary batteries or lithium ion polymer secondary batteries are preferred.

[0070] Hereinafter, the present invention will be described in more detail by way of examples. However, the embodiments described in the specification and the configurations described in the accompanying drawings are only the most preferred embodiments of the present invention and do not represent the entire technical concept of the present invention. It should be understood that multiple equivalents and variants may exist to replace them when submitting this application.

[0071] Examples and Comparative Examples

[0072] Example 1

[0073] Powdered polyvinylidene fluoride (PVDF) homopolymer (KF-1100, Kureha, weight average molecular weight 280000 g / mol) was granulated into cylindrical pellets with an average diameter of 3 mm. The granulated PVDF was mixed in NMP (N-methyl-2-pyrrolidone) to 25% by weight, and then stirred at 25°C for 2 hours using a stirrer (IK R010).

[0074] Figure 1 The results of observation after filtering the solution after the stirring process through a 200-mesh filter are shown. Figure 1 It can be seen that the granulated PVDF dissolved in the solvent NMP passes through the filter with almost no filtered material. It can be seen that the granulated PVDF is efficiently dissolved while almost no floating matter is generated.

[0075] Example 2

[0076] Powdered polyvinylidene fluoride (PVDF) homopolymer (KF-1100 and KF-7200 mixed in a ratio of 1:1, Kureha Co., Ltd.) was pelletized into cylindrical pellets with an average diameter of 3 mm. The pelletized PVDF was mixed in NMP (N-methyl-2-pyrrolidone) to 20% by weight and then stirred at 25°C for 2 hours using a stirrer (IK Co., Ltd. R010).

[0077] Example 3

[0078] Powdered polyvinylidene fluoride (PVDF) homopolymer (KF-1100, Kureha, weight average molecular weight of 280000 g / mol) was granulated into cylindrical pellets with an average diameter of 2 mm. In addition, powdered polyvinylidene fluoride (PVDF) homopolymer (KF-7200, Kureha, weight average molecular weight of 630000 g / mol) was granulated into cylindrical pellets with an average diameter of 4 mm. Each granulated PVDF was mixed in NMP (N-methyl-2-pyrrolidone) to 20% by weight at a mixing ratio of 1.5:1, and then stirred at 25°C for 2 hours using a stirrer (IK R010).

[0079] Comparative Example 1

[0080] After mixing powdered polyvinylidene fluoride (PVDF) homopolymer (KF-1100, Kureha, weight average molecular weight 280000 g / mol) in NMP (N-methyl-2-pyrrolidone) to 25 wt%, the mixture was stirred at 25°C for 2 hours using a stirrer (IK R010).

[0081] Figure 2 The results of observation after filtering the solution after the stirring process through a 200-mesh filter are shown. Figure 2 , it can be seen that the powdered PVDF dissolved in the solvent NMP passes through the filter and has a lot of filtered material. It can be seen that even after the stirring used in the dissolution process, relatively many impurities remain in the powdered PVDF. This is because a lot of suspended matter is generated during the dissolution, resulting in reduced solubility.

[0082] Comparative Example 2

[0083] After mixing powdered polyvinylidene fluoride (PVDF) homopolymer (KF-7200, Kureha, weight average molecular weight 630000 g / mol) in NMP (N-methyl-2-pyrrolidone) to 20 wt%, the mixture was stirred at 25°C for 2 hours using a stirrer (IK R010).

[0084] Example 4: Preparation of positive electrode composite

[0085] With respect to 100 parts by weight of the binder solution prepared according to Example 1, 450 parts by weight of lithium cobalt composite oxide as positive electrode active material particles and 25 parts by weight of carbon black as a conductive material were mixed to prepare a positive electrode active material slurry. The prepared positive electrode active material slurry was applied to a positive electrode collector, dried, and rolled to prepare a positive electrode composite. An aluminum (Al) film having a thickness of 20 μm was used as a positive electrode collector.

[0086] Figure 3 The results of observing the cross section of the positive electrode composite layer according to Example 4 are shown. Figure 3 It can be seen that positive electrode active material particles having a shape close to a spherical shape are dispersed, and have a structure in which the binder according to Example 1 and the conductive material are filled between the positive electrode active material particles. Figure 3 It was confirmed that the positive electrode active material particles were uniformly dispersed in the layer, and the void portion filled with the binder and the conductive material had a relatively small void size.

[0087] also, Figure 4 is the result of observing the cross section of the positive electrode composite layer according to Example 4 using energy dispersive spectroscopy (EDS). Figure 4 In the cross section, fluorine (F) was mapped, and it was confirmed that the PVDF binder portion filled between the positive electrode active material particles appeared green.

[0088] Example 5: Preparation of negative electrode composite

[0089] Relative to 100 parts by weight of the binder solution prepared according to Example 3, 95 parts by weight of carbon powder as negative electrode active material particles and 3 parts by weight of carbon black as a conductive material were mixed to prepare a negative electrode active material slurry. The prepared negative electrode active material slurry was applied to a negative electrode collector, dried and rolled to prepare a negative electrode composite. A copper (Cu) film having a thickness of 90 μm was used as a negative electrode collector.

[0090] Comparative Example 3: Preparation of positive electrode composite

[0091] Using the binder solution prepared according to Comparative Example 1, a positive electrode composite was prepared in the same manner as in Example 4.

[0092] Figure 5 This is the observation result of the cross section of the positive electrode composite layer according to Comparative Example 3. Figure 5 It can be seen that positive electrode active material particles having a shape close to a spherical shape are dispersed, and the binder according to Comparative Example 1 is filled between the positive electrode active material particles. Figure 5 As shown, the positive electrode active material particles are not uniformly dispersed, and the voids filled with the binder are mixed with relatively large and relatively small voids.

[0093] also, Figure 6 The results of observing the cross section of the positive electrode composite layer according to Comparative Example 3 using energy dispersive spectroscopy (EDS) are shown. Figure 6 In the cross section, fluorine (F) was mapped, and it was confirmed that the PVDF binder portion filled between the positive electrode active material particles appeared green.

[0094] Comparative Example 4: Preparation of negative electrode composite

[0095] Using the binder solution prepared according to Comparative Example 2, a positive electrode composite was prepared in the same manner as in Example 5.

[0096] Experimental Example 1: Evaluation of Adhesion

[0097] The electrode composites prepared in Example 4 and Comparative Example 3 were evaluated for adhesion. In the evaluation of adhesion, the adhesion between the electrode collector and the positive electrode composite layer mixed with active material, conductive material and binder was evaluated. Specifically, the average thickness of the coating film of the electrode composite layer was 90 μm, and the sample was prepared to be 2 cm wide and 20 cm long. The results are shown in Table 1.

[0098] [Table 1]

[0099] Instance number Adhesion force (N / m) Example 4 120.1 Comparative Example 3 85.8

[0100] Referring to Table 1, Example 4 showed an adhesion of 120.1 N / m, and Comparative Example 3 showed an adhesion of 85.8 N / m. That is, the adhesion of the electrode composite according to Example 4 was improved by nearly 40% compared with Comparative Example 3. It was thus confirmed that the adhesion of the electrode binder can be significantly improved through the PVDF granulation process.

[0101] Experimental Example 2: Capacity Retention Evaluation

[0102] Batteries were fabricated using the electrode composites prepared in Examples 4 and 5, respectively, and the electrode composites prepared in Comparative Examples 3 and 4, respectively.

[0103] Specifically, a unit cell was assembled by placing a polyolefin-based separator between the positive electrode composite according to Example 4 and the negative electrode composite according to Example 5. Then, an electrolyte (ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC)=3 / 2 / 5 (volume ratio) and lithium hexafluorophosphate (LiPF6) was 1 M) was injected to prepare a secondary battery (Example battery).

[0104] In addition, using the positive electrode composite according to Comparative Example 3 and the negative electrode composite according to Comparative Example 4, a secondary battery (Comparative Example battery) was manufactured by the same method.

[0105] Each battery was charged and discharged, and the capacity retention rate according to the number of charge and discharge cycles was evaluated. Specifically, the capacity at the first discharge was set to 100%, and the capacity change according to the charge and discharge cycle was relatively evaluated. The conditions of the sample were the same as those of Experimental Example 1. The evaluation results are shown in Table 2, and the capacity retention rate was relatively evaluated after the charge and discharge cycles were repeated for each number of times.

[0106] [Table 2]

[0107]

[0108] Referring to Table 2, in the example battery, after repeated charge and discharge 100 times, the capacity retention rate relative to the initial stage was 96.1%, and after repeated charge and discharge 400 times, the capacity retention rate relative to the initial stage was 91.2%. On the other hand, in the comparative example battery, after repeated charge and discharge 100 times, the capacity retention rate relative to the initial stage was 95.7%, and after repeated charge and discharge 400 times, the capacity retention rate relative to the initial stage remained at 89.5%. That is, in the example battery, more than 90% of the capacity was maintained even after repeated charge and discharge 400 times, but in the comparative example battery, it can be seen that the capacity dropped to less than 90% under the same conditions.

Claims

1. A method for manufacturing an electrode binder, the method comprising: The step of dissolving the granulated polyvinylidene fluoride in a solvent, wherein the granulated polyvinylidene fluoride is in a form in which powdery particles are aggregated to form granules, and wherein the average diameter of the granules is in a range of greater than 1 mm to less than or equal to 5 mm, The powdery particles contain at least one of the following: a weight average molecular weight of 2.0×10 5 ~7.5×10 5 The first powder particles; and a weight average molecular weight of 7.5×10 5 ~2.5×10 6 The second powder particles, The polyvinylidene fluoride is one or more selected from the following: polyvinylidene fluoride homopolymer, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polyvinylidene fluoride-co-tetrafluoroethylene, polyvinylidene fluoride-co-trifluoroethylene, polyvinylidene fluoride-co-chlorotrifluoroethylene and polyvinylidene fluoride-co-ethylene. 2 . The method according to claim 1 , wherein the length ratio of the major axis to the minor axis of the polyvinylidene fluoride particles is in the range of 20:1 to 1:

1.

3. The method of claim 1, wherein the solvent is a water-soluble solvent having a polar group. 4 . The method of claim 1 , wherein the solvent is at least one selected from the group consisting of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane and water. 5 . The method of claim 1 , wherein the content of polyvinylidene fluoride dissolved in the solvent is in the range of 1 wt % to 25 wt %. 6 . The method according to claim 1 , further comprising the step of adding a conductive material during or after the step of dissolving the particle-formed polyvinylidene fluoride in the solvent.

7. An electrode composite, comprising: an electrode current collector; and an electrode composite layer coated on one or both sides of the electrode current collector, wherein the electrode composite layer comprises: a particulate active material; a binder comprising polyvinylidene fluoride; and a conductive material, The electrode composite layer is filled with a particle-shaped active material, and the gaps between the active material particles are filled with a binder and a conductive material. wherein the voids have a porosity of 15% to 35% by volume, and The average diameter of the voids is 0.01 to 1 mm. The binder is prepared by the method of claim 1, provided that the solvent is removed from the electrode composite layer by a drying process.

8. The electrode composite according to claim 7, wherein the particulate active material comprises: first particles having an average particle size in the range of 5 to 10 μm; and second particles having an average particle size in the range of 100 to 200 μm, based on a cross section of the electrode composite layer. The ratio of the areas occupied by the first particles to the areas occupied by the second particles is in the range of 1:1 to 10:

1.

9. The electrode composite according to claim 7, wherein the coating film of the electrode composite layer has an average thickness of 50 to 150 μm, and For a sample having a width of 2 cm and a length of 20 cm, the adhesion between the electrode current collector and the composite layer mixed with the active material, the conductive material and the binder is 100 N / m or more.