Preparation method of doped ZnO catalyst and preparation method of synthesizing higher alcohol using the same

By doping Ga or Cu in a low copper content in Cu/ZnO catalyst, doping ZnO catalysts is solved, and the problem of low selectivity of advanced alcohols in existing catalysts is achieved, and the proportion of higher alcohols and catalyst activity of higher alcohols is achieved. It is suitable for The CO hydrogenation reaction on the fixed bed is in line with the development direction of green chemical industry.

CN113856687BActive Publication Date: 2024-11-22TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111300875.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-04
Publication Date
2024-11-22
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

Existing Cu/ZnO catalysts perform poorly in selectivity of higher alcohols, and usually require the addition of Fischer-Tropsch to increase the product proportion of higher alcohols, while the proportion of higher alcohols is low, and the main product is methanol.

Method used

Using Cu or Ga doped ZnO catalyst with low copper content, copper or gallium doped into the ZnO lattice through co-precipitation method or hydrothermal synthesis method, a new catalyst was designed to increase the product ratio of higher alcohols and carried out on a fixed bed. CO hydrogenation reaction.

Benefits of technology

It has achieved a high proportion of high alcohols (>40%) and high activity of catalysts, and does not use any additives or Fischer-Tropsch elements. It has a simple process and low cost, which is in line with the development trend of green chemical industry.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The embodiment of the present invention provides a method for preparing a doped ZnO catalyst for synthesizing higher alcohols by hydrogenation of CO on a fixed bed, comprising the following steps: providing a precipitant and a first solvent to form a first solution, wherein the concentration of the precipitant is 1 to 5 mol / L; providing one of a Cu salt or a Ga salt, a Zn salt, and a second solvent to form a second solution, wherein the molar ratio of Cu to Zn is less than 0.05, and the molar ratio of Ga to Zn is less than 0.1; subjecting the first solution and the second solution to a precipitation or hydrolysis process at 50 to 90°C to obtain a precipitate, washing and drying the precipitate to obtain a precursor sample, calcining at 300 to 500°C for 3 to 5 hours, and obtaining a final Cu or Ga doped ZnO catalyst. In addition, the embodiment of the present invention also provides a method for preparing a doped ZnO catalyst for synthesizing higher alcohols. The present invention belongs to the field of catalysis and chemical engineering technology. In the method of the present invention, the proportion of higher alcohols is high, and the catalyst activity is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysis and chemical engineering, and in particular to a method for preparing a doped ZnO catalyst and a method for synthesizing higher alcohols using the same. Background Art

[0002] As basic substances, carbon monoxide and hydrogen have a wide range of sources. The conversion of coal or natural gas into synthesis gas has become a mature technology in industry. The synthesis of low-carbon mixed alcohols from synthesis gas is a very popular research topic in the current C1 chemistry field. The technology of synthesizing low-carbon alcohols from synthesis gas is an important direction for the synthesis of liquid fuels, oil additives and bulk chemicals through non-petroleum routes. The overall process flow of this technology is that synthesis gas is used to synthesize low-carbon mixed alcohols mainly composed of C1-C6 under the action of a multiphase catalyst, among which alcohols containing two carbon atoms or more are called higher alcohols. This process has the characteristics of low production cost, atom economy and strong operational feasibility. Higher alcohols have broad application prospects, and alcohols with high industrial value can be obtained after separation. In addition, higher alcohols can also be used as clean fuels and general chemical solvents. At present, a variety of catalyst systems for synthesizing higher alcohols have been developed, which can be roughly divided into three categories: (1) FT synthesis catalyst, with straight-chain mixed alcohols as the main product, and the product distribution conforms to the ASF distribution; (2) Mo-based catalyst, the product contains 70-80% alcohol and 15-30% hydrocarbons; (3) modified methanol synthesis catalyst, the product is mainly branched alcohol (isobutanol). The technology of synthesizing higher alcohols from syngas has opened up a diversified product route for producing oxygenated liquid fuels, oil additives and high-value-added alcohol chemicals using coal-based syngas as raw materials. Its economic efficiency is better than the current methanol synthesis technology, and it can be used to gradually implement alternative methanol synthesis technology to produce high-value-added fuel alcohols or chemical alcohols. It has broad promotion and application prospects in effectively solving the problem of methanol overproduction, avoiding methanol market risks and producing alternative fuels. After the implementation of industrial production, this technology will form an industrial chain in my country that uses coal as the source and synthesizes alternative fossil fuels and chemical alcohols through non-petroleum routes, creating more employment opportunities and driving the development of related alcohol chemical secondary processing industries.

[0003] The modified low-temperature methanol synthesis catalyst mainly includes Cu / ZnO / Al 2 O 3 and Cu / ZnO / Cr 2 O 3 , the reaction conditions are generally 220-290℃ and 4-6Mpa. It is generally believed that Cu-Zn based catalysts are bifunctional catalysts, Cu is the main active center, which can activate the dissociative adsorption of H 2; ZnO is a dispersed active component, which can prevent the sintering of active components. The preparation process of Cu-Zn-based catalysts is simple, the price is low, the reaction conditions are mild, the reaction activity and total alcohol selectivity are high, but the proportion of higher alcohols is low, and the alcohol product is mainly methanol. The loading amount of copper, the active component, in these Cu-Zn-based catalysts is more than 10wt%, and when the copper-zinc ratio is 1:1, their proportion of higher alcohols is very low, and the alcohol product is mainly methanol. Other Fischer-Tropsch elements such as Fe, Co, Ni, etc. are added to the copper-containing catalyst with significantly improved selectivity for higher alcohols.

[0004] In summary, the catalytic product of general Cu / ZnO catalysts is mainly methanol, and the content of copper components is above 5wt%, while the proportion of higher alcohols is relatively low. In catalysts with higher selectivity for higher alcohols, at least one Fischer-Tropsch element is added on the basis of copper and zinc components. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a Cu or Ga doped ZnO catalyst capable of synthesizing higher alcohols and a method for preparing higher alcohols using a doped ZnO catalyst, wherein the proportion of higher alcohols is relatively high and no Fischer-Tropsch elements are used.

[0006] The inventors of the present invention have found no reports on the use of Ga-doped ZnO catalysts for the production of higher alcohols from syngas, and no reports on the use of low-loaded Cu in doping ZnO catalysts to synthesize higher alcohols. Therefore, this patent uses Cu or Ga metal-doped ZnO catalysts to electronically regulate the ZnO catalysts to achieve the synthesis of higher alcohols on ZnO catalysts.

[0007] The copper content in the Cu or Ga-doped ZnO catalyst prepared in the embodiment of the present invention is very low, and no additives and Fischer-Tropsch elements are added. It shows high activity and excellent proportion of higher alcohols in the CO hydrogenation reaction, and the synergistic effect of copper-zinc or gallium-zinc is strong. The catalyst synthesis method described in the embodiment of the present invention is relatively simple, and metallic copper or gallium is doped into the ZnO lattice by coprecipitation or hydrothermal synthesis. The synthesized catalyst has a uniform flower-like or nanosheet morphology, wherein the doping amount of Cu in 1 mol ZnO is 1 to 4 mol%. The doping amount of Ga is 1 to 10 mol%.

[0008] In the embodiments of the present invention, the preparation method of the catalyst has the advantages of simple process, low cost, high catalytic performance, etc., which conforms to the development trend of green chemical industry; and has broad application prospects in the field of CO catalytic conversion into important chemicals.

[0009] The embodiments of the present invention provide a preparation and application of a Cu or Ga-doped ZnO catalyst for synthesizing higher alcohols on a fixed bed. Based on the current research progress of catalysts for preparing low-carbon alcohols from synthesis gas, the present invention uses ZnO as the main active ingredient of the catalyst, doping a very small amount of copper or gallium to enhance the interaction between the two, and designs a new Cu or Ga-doped ZnO catalyst without adding any additives or Fischer-Tropsch elements. The Cu-doped ZnO catalyst has a lower copper content than the traditional catalyst, and copper ions enter the ZnO lattice. The preparation method of the present invention can produce a new higher alcohol catalyst with simple components, easy operation, good catalyst activity, a high proportion of higher alcohols, and high catalytic efficiency.

[0010] In one aspect of the present invention, a Cu or Ga doped ZnO catalyst for preparing higher alcohols by hydrogenation of CO on a fixed bed is provided. The preparation method thereof can be carried out by a coprecipitation method or a hydrothermal synthesis method. The main preparation process thereof is as follows:

[0011] (1) selecting a suitable precipitant such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, sodium oxalate, ammonia water, ammonium carbonate, urea or ammonium bicarbonate, adding a suitable amount of solvent (e.g., deionized water) to dissolve the precipitant, and placing the precipitant in a magnetic stirrer and stirring the precipitant for a period of time; the concentration of the precipitant in the formed solution is 1 to 5 mol / L, and a first solution A is obtained;

[0012] (2) Weighing a certain proportion of Cu salt (copper nitrate, copper sulfate, copper chloride, copper citrate) and Zn salt (such as zinc nitrate, zinc sulfate, zinc acetate, zinc chloride), adding an appropriate amount of solvent (such as deionized water) to dissolve them, and placing them in a magnetic stirrer and stirring for 20 minutes (min); obtaining a second solution B1, wherein the molar ratio of copper to zinc is less than 0.05;

[0013] (3) Weighing Ga salt (gallium nitrate, gallium sulfate, gallium acetate, gallium chloride) and Zn salt (such as zinc nitrate, zinc sulfate, zinc acetate, zinc chloride) in a certain proportion, adding an appropriate amount of solvent (such as deionized water) to dissolve them, and placing them in a magnetic stirrer and stirring for 20 minutes; obtaining another second solution B2, in which the molar ratio of gallium to zinc is less than 0.1;

[0014] (4) subjecting the first solution A and the second solution B to a precipitation or hydrolysis process at 50 to 90° C. to obtain a precipitate, and washing and drying the precipitate to obtain a precursor sample;

[0015] (5) Calcine the precursor sample at 300-500° C. for 3-5 hours (h) to obtain the final Cu or Ga-doped ZnO catalyst.

[0016] In another aspect of the present invention, a method for synthesizing higher alcohols using a doped ZnO catalyst is provided. The doped ZnO catalyst used in the preparation method is prepared by the above-mentioned method for preparing the ZnO catalyst, and specifically comprises the following steps: grinding, tableting, crushing, and sieving the doped ZnO catalyst, and then filling it in a fixed bed and fixing its position with a filler, and reducing the doped ZnO catalyst in a hydrogen atmosphere, for example, and reacting it in the fixed bed. The conditions for using the doped ZnO catalyst in the fixed bed catalytic CO hydrogenation reaction are uniformly: pressure 4-6 MPa, temperature 200-400°C, GHSV (volume space velocity) = 3000-9000h -1 , H 2 / CO=1~2.

[0017] After the catalytic reaction of the catalyst is stable, the conversion rate of carbon monoxide (CO) is 10-70%, and the proportion of higher alcohols in the obtained product is greater than 40%.

[0018] In the embodiments of the present invention, a method for preparing higher alcohols by hydrogenating CO on a fixed bed using a doped ZnO catalyst is provided, which has a high proportion of higher alcohols, good catalyst activity, a simple preparation method, and good industrial prospects. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further specifically described below through examples. The following description of the embodiments of the present invention is intended to explain the overall concept of the present invention, and should not be construed as a limitation of the present invention.

[0020] In the background technology section, the shortcomings of Cu-doped ZnO catalysts are discussed. One is that when the Cu doping amount is above 5wt%, the catalytic product is mainly methanol, while the hope is to obtain more higher alcohols; the second is that in order to obtain more higher alcohols, at least one Fischer-Tropsch element is often used on the basis of the zinc-copper components.

[0021] In view of this technical problem, an embodiment of the present invention provides a method for preparing a doped ZnO catalyst, wherein the doped ZnO catalyst is used for synthesizing higher alcohols by hydrogenation of CO on a fixed bed, and the preparation method comprises the following steps:

[0022] Providing a precipitant and a first solvent to form a first solution, wherein the concentration of the precipitant in the first solution is 1 to 5 mol / L;

[0023] Providing one of a Cu salt or a Ga salt, a Zn salt, and a second solvent to form a second solution, wherein the molar ratio of Cu to Zn in the second solution is less than 0.05, and the molar ratio of Ga to Zn is less than 0.1;

[0024] subjecting the first solution and the second solution to a precipitation or hydrolysis process at 50 to 90° C. to obtain a precipitate, and washing and drying the precipitate to obtain a precursor sample;

[0025] The precursor sample is calcined at 300-500° C. for 3-5 hours to obtain the final Cu or Ga doped ZnO catalyst.

[0026] In one example, the precipitant includes any one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, sodium oxalate, ammonia water, ammonium carbonate, urea and ammonium bicarbonate, or any combination thereof.

[0027] In another example, the Cu salt includes any one of copper nitrate, copper sulfate, copper chloride and copper citrate or any combination thereof; or the Ga salt includes any one of gallium nitrate, gallium sulfate, gallium acetate and gallium chloride or any combination thereof. Optionally, the Zn salt includes any one of zinc nitrate, zinc sulfate, zinc acetate and zinc chloride or any combination thereof. At least one of the first solvent and the second solvent includes deionized water.

[0028] It can be understood that the precipitants, Cu salts, Ga salts and Zn salts are merely shown as some common examples and are not exhaustive.

[0029] In a further example, the molar ratio of Cu to Zn is 0.01-0.04 (eg, 0.01, 0.02, 0.03 or 0.04), and the molar ratio of Ga to Zn is 0.01-0.1 (eg, 0.01, 0.03, 0.05, 0.07 or 0.1).

[0030] In some examples, a precipitant is added to a first solvent to dissolve it, and then placed in, for example, a magnetic stirrer for stirring to form the first solution; a Cu salt or a Ga salt and a Zn salt are added to a second solvent to dissolve it, and then placed in a magnetic stirrer for stirring to obtain a second solution.

[0031] It can be understood that the above preparation method adopts co-precipitation method or hydrothermal synthesis method, and of course any other known suitable method can also be adopted.

[0032] In addition, an embodiment of the present invention further provides a method for preparing higher alcohols by using a doped ZnO catalyst, wherein the doped ZnO catalyst is prepared by the above-mentioned preparation method, and the method for preparing higher alcohols by CO hydrogenation on a fixed bed using a doped ZnO catalyst comprises the following steps:

[0033] The doped ZnO catalyst is ground, tableted, crushed, and sieved, and then filled in a fixed bed and fixed in position with a filler, and the doped ZnO catalyst is reduced in a hydrogen atmosphere and reacted in the fixed bed, wherein the conditions for the doped ZnO catalyst to be used in the fixed bed catalytic CO hydrogenation reaction are: pressure 4-6MPa, temperature 200-400°C (optionally 250-320°C), GHSV=3000-9000h -1 (optionally 5000~8000h -1 ), H 2 / CO=1~2.

[0034] In some examples, after the catalytic reaction of the doped ZnO catalyst is stabilized, the conversion rate of carbon monoxide is 10-70%, and the proportion of higher alcohols in the obtained product is greater than 40%.

[0035] The following only shows a part of the embodiments of the present invention, which is only for illustrative purposes; those skilled in the art may understand other feasible embodiments of the present invention, which will not be described here.

[0036] Example 1

[0037] Weigh zinc nitrate and dissolve it in 200 mL of deionized water, then add copper nitrate and stir under magnetic stirring for 20 min to form a copper-zinc salt solution, where n(Cu):n(Zn)=0.01;

[0038] Then, 1.6 M sodium carbonate was dissolved in 200 mL of deionized water, stirred under magnetic stirring for 20 min, and then placed in a water bath and heated to 20° C. to form a sodium carbonate solution;

[0039] Sodium carbonate solution and copper-zinc salt solution are respectively added dropwise into a reaction vessel (e.g., a three-necked flask) to maintain pH=6.5, and stirred continuously to form a uniform and stable precipitate at 65° C. After further aging (e.g., 6 hours), the precipitate is filtered and washed to obtain a precipitate;

[0040] The precursor sample was dried at 100 °C overnight to obtain the precursor sample, which was then calcined at 330 °C for 3 h in a muffle furnace to obtain the final Cu-doped ZnO catalyst;

[0041] The Cu-doped ZnO catalyst was ground, tableted, crushed and sieved to obtain catalyst particles of 40 to 60 mesh. The Cu-doped ZnO catalyst was loaded into a fixed bed reactor and fixed with fillers. The Cu-doped ZnO catalyst was first heated in H 2 atmosphere, and then at 300°C, 4MPa, H 2 / CO=1,GHSV=6000h -1The activity of the reaction was evaluated under the conditions of . The reaction activity evaluation results are shown in Table 1. The proportion of higher alcohols is the percentage of C2+ alcohols in the alcohol product.

[0042] Example 2

[0043] Dissolve zinc nitrate in 200 mL of deionized water, then add copper nitrate, and stir under magnetic stirring for 20 min to form a copper-zinc salt solution, wherein n(Cu):n(Zn)=0.04;

[0044] Then, 3 mol / L urea was dissolved in 200 mL of deionized water, stirred for 20 min under magnetic stirring, and then placed in a water bath and heated to 20° C. to form a urea solution;

[0045] The copper-zinc salt solution and the urea solution are formed into a uniform and stable solution, heated at 90°C for 8 hours, and filtered and washed to obtain a precipitate;

[0046] The precursor sample was dried at 100°C overnight to obtain a precursor sample, and then calcined at 330°C for 3h in a muffle furnace to obtain the final Cu-doped ZnO catalyst.

[0047] The Cu-doped ZnO catalyst was ground, tableted, crushed and sieved to obtain catalyst particles of 40 to 60 mesh. The Cu-doped ZnO catalyst was loaded into a fixed bed reactor and fixed with fillers. The Cu-doped ZnO catalyst was first heated in H 2 atmosphere, and then at 290°C, 4MPa, H 2 / CO=2,GHSV=6000h -1 The activity of the reaction was evaluated under the conditions of . The reaction activity evaluation results are shown in Table 1. The proportion of higher alcohols is the percentage of C2+ alcohols in the alcohol product.

[0048] Example 3

[0049] Dissolve zinc nitrate in 200 mL of deionized water, then add gallium nitrate and stir under magnetic stirring for 20 min to form a gallium zinc salt solution, wherein n(Ga):n(Zn)=0.01;

[0050] Then, 1.6 M sodium carbonate was dissolved in 200 mL of deionized water, stirred under magnetic stirring for 20 min, and then placed in a water bath and heated to 20° C. to form a sodium carbonate solution;

[0051] Sodium carbonate solution and zinc gallium salt solution are added dropwise into a three-necked flask to maintain pH=6.5, and stirred continuously to form a uniform and stable precipitate, and then aged (for example, for 6 hours) and then filtered and washed to obtain the precipitate;

[0052] The precursor sample was dried at 100°C overnight to obtain a precursor sample, which was then calcined at 330°C in a muffle furnace for 3 h to obtain the final Ga-doped ZnO catalyst.

[0053] The Ga-doped ZnO catalyst was ground, tableted, crushed and sieved to obtain catalyst particles of 40 to 60 mesh. The Ga-doped ZnO catalyst was loaded into a fixed bed reactor and fixed with fillers. The Ga-doped ZnO catalyst was first heated in H 2 atmosphere, and then at 280°C, 4MPa, H 2 / CO=2,GHSV=6000h -1 The activity of the reaction was evaluated under the conditions of . The reaction activity evaluation results are shown in Table 1. The proportion of higher alcohols is the percentage of C2+ alcohols in the alcohol product.

[0054] Example 4

[0055] Dissolve zinc nitrate in 200 mL of deionized water, then add gallium nitrate, and stir under magnetic stirring for 20 minutes to form a gallium zinc salt solution, wherein n(Ga):n(Zn)=0.04;

[0056] Then, 3 mol / L urea was dissolved in 200 mL of deionized water, stirred for 20 min under magnetic stirring, and then placed in a water bath and heated to 20° C. to form a urea solution;

[0057] Then, the gallium zinc salt solution and the urea solution were formed into a uniform and stable solution, hydrothermally heated at 90°C for 8 hours, filtered and washed to obtain a precipitate, dried at 100°C overnight to obtain a precursor sample, and then calcined at 330°C in a muffle furnace for 3 hours to obtain the final Ga-doped ZnO catalyst;

[0058] The Ga-doped ZnO catalyst was ground, tableted, crushed and sieved to obtain catalyst particles of 40 to 60 mesh. The Ga-doped ZnO catalyst was loaded into a fixed bed reactor and fixed with fillers. The Ga-doped ZnO catalyst was first heated in H 2 atmosphere, and then at 300°C, 4MPa, H 2 / CO=1,GHSV=8000h -1 The activity of the reaction was evaluated under the conditions of , and the results of the reaction activity evaluation are shown in Table 1. The proportion of higher alcohols is C 2+ The percentage of alcohol.

[0059] Table 1 Evaluation results of catalyst reaction activity in embodiments 1-4

[0060] Example CO conversion rate (%) Higher alcohol proportion (%) 1 62.84 46.08 2 18.06 69.89 3 15.75 65.78 4 16.23 55.31

[0061] In an embodiment of the present invention, at least one of the advantages described in the following aspects is achieved: ZnO is used as the main component of the catalyst, and a small amount of copper or gallium is doped to enhance the interaction between the two;

[0062] The copper content in the copper-doped ZnO catalyst is very low (<0.05 mol), and the gallium content in the gallium-doped ZnO catalyst is less than 0.1 mol, and no additives or Fischer-Tropsch elements are added;

[0063] Cu or Ga doped ZnO catalysts show good activity and excellent higher alcohol ratio in CO hydrogenation reaction;

[0064] The Cu or Ga doped ZnO catalyst is prepared by a co-precipitation method or a hydrothermal synthesis method.

[0065] Although some embodiments of the general inventive concept of the present disclosure have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the general inventive concept of the present disclosure, the scope of which is defined by the claims and their equivalents.

Claims

1. A method for preparing a doped ZnO catalyst, wherein the method adopts a hydrothermal synthesis method to prepare a doped ZnO catalyst. The following steps are involved: Providing a precipitant and a first solvent to form a first solution, wherein the concentration of the precipitant in the first solution is 1-5 mol / L; Providing a Ga salt, a Zn salt and a second solvent to form a second solution, wherein the molar ratio of Ga to Zn in the second solution is 0.01 to 0.1, The first solution and the second solution are subjected to a hydrolysis process at 50-90° C. to obtain a precipitate, and the precipitate is washed and dried to obtain a precursor sample. Calcinate at 300-500°C for 3-5 hours to obtain the final Ga-doped ZnO catalyst. The Ga-doped ZnO catalyst finally obtained has ZnO as its main active ingredient, and the synthesized catalyst has a uniform flower-like or nanosheet morphology, so that when the final Ga-doped ZnO catalyst is used for CO hydrogenation synthesis of higher alcohols on a fixed bed, the conversion rate of CO is 10-70%, and the proportion of the higher alcohol in the obtained product is greater than 40%. In the process of preparing the Ga-doped ZnO catalyst, the metal gallium is doped into the ZnO lattice by a hydrothermal synthesis method to electronically control the ZnO without adding any additives or Fischer-Tropsch elements. When doping with metallic gallium, the doping amount of Ga in 1 mol of ZnO is 1-10 mol%, and the gallium content in the Ga-doped ZnO catalyst finally obtained is less than 0.1 mol.

2. The method for preparing the doped ZnO catalyst according to claim 1, in, The precipitant includes any one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, sodium oxalate, ammonia water, ammonium carbonate, urea and ammonium bicarbonate, or any combination thereof.

3. The method for preparing the doped ZnO catalyst according to claim 2, in, The Ga salt includes any one of gallium nitrate, gallium sulfate, gallium acetate and gallium chloride, or any combination thereof.

4. The method for preparing the doped ZnO catalyst according to claim 3, in, The Zn salt includes any one of zinc nitrate, zinc sulfate, zinc acetate and zinc chloride or any combination thereof.

5. The method for preparing the doped ZnO catalyst according to claim 4, in, At least one of the first solvent and the second solvent includes deionized water.

6. A method for preparing a doped ZnO catalyst according to any one of claims 2 to 5, in, Adding a precipitant to the first solvent to dissolve it, and placing it in a magnetic stirrer to stir to form the first solution; One of the Ga salts and the Zn salt are added to the second solvent to dissolve them, and then placed in a magnetic stirrer to stir to obtain a second solution. When the precipitant is urea, the hydrolysis condition in the hydrothermal synthesis method is hydrothermal treatment at 90° C. for 8 h.

7. A method for synthesizing higher alcohols using a doped ZnO catalyst, wherein the doped ZnO catalyst is prepared by the method according to any one of claims 1 to 6, and the method for synthesizing higher alcohols by CO hydrogenation on a fixed bed using the doped ZnO catalyst The following steps are involved: The doped ZnO catalyst is ground, tableted, crushed, and sieved, and then filled in a fixed bed and fixed in position with a filler, and the doped ZnO catalyst is reduced and reacted in the fixed bed, wherein the conditions for the doped ZnO catalyst to be used in the fixed bed catalytic CO hydrogenation reaction are: pressure 4-6 MPa, temperature 200-400°C, GHSV=3000-9000 h -1 , H 2 / CO=1~2.

8. The method for synthesizing higher alcohols using a doped ZnO catalyst according to claim 7, in, The doped ZnO catalyst is reduced in a hydrogen atmosphere; After the catalytic reaction of the doped ZnO catalyst is stabilized, the conversion rate of carbon monoxide is 10-70%, and the proportion of higher alcohols in the obtained product is greater than 40%.