A method for recovering battery-grade lithium carbonate from lithium-ion battery positive electrode material

The ammonia reduction roasting method is used to process lithium-ion battery cathode materials under anaerobic conditions, which solves the problems of safety risks in the use of hydrogen and lengthy impurity removal processes, achieves the recovery of high-purity lithium carbonate and the effective utilization of transition metal resources, and simplifies the process process.

CN114256526BActive Publication Date: 2024-10-11SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111403574.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-22
Publication Date
2024-10-11
Estimated Expiration
2041-11-22

AI Technical Summary

Technical Problem

The existing technology uses hydrogen as a reducing agent in the recycling of lithium-ion battery cathode materials, which poses explosion safety risks and increases process costs. Moreover, the lengthy impurity removal process makes it difficult to obtain high-purity lithium carbonate.

Method used

Using the ammonia reduction roasting method, the waste lithium-ion battery cathode material is reacted with an ammonia-generating agent under anaerobic conditions to generate a lithium-rich aqueous solution, and battery-grade lithium carbonate is obtained through heating, concentration and chemical precipitation, avoiding the use of hydrogen. and lengthy impurity removal process.

Benefits of technology

It has achieved safe and low-cost recycling of lithium-ion battery cathode material resources and obtained high-purity lithium carbonate, which is suitable for a variety of lithium-transition metal oxide lithium-ion batteries, simplifying the process chain and reducing the dosage of chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114256526B_ABST
    Figure CN114256526B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for recovering battery-grade lithium carbonate from positive electrode materials of lithium-ion batteries; the method comprises the following steps: discharging the positive electrode materials of lithium-ion batteries, then disassembling the positive electrode sheets, removing the binder by high-temperature pyrolysis, and separating and enriching the positive electrode materials; subjecting the enriched positive electrode materials to ammonia reduction conversion, and then washing and filtering to obtain a lithium-rich aqueous solution; heating and concentrating the filtrate, adding sodium carbonate to precipitate, and recovering the battery-grade lithium carbonate after filtering. The present invention uses an ammonia reduction roasting method to achieve the selective recovery of lithium resources in the positive electrode materials, reducing the large-scale use of reducing agents such as strong acids, and also recovering high-purity transition metal elements or oxides, thereby achieving the effective recovery of metal resources in the positive electrode materials. The method adopts the ammonia reduction conversion process widely used in industry, uses less chemical agents, and achieves the recovery of battery-grade lithium carbonate, which has broad industrial application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource processing of waste lithium-ion batteries, and in particular to a method for recovering battery-grade lithium carbonate from positive electrode materials of lithium-ion batteries; in particular, it relates to a method for recovering battery-grade lithium carbonate from positive electrode materials of lithium-transition metal oxide type lithium-ion batteries. Background Art

[0002] With the rapid development of new energy technologies, the lithium-ion battery industry has entered a period of ultra-high-speed expansion. Its huge production capacity needs have had a huge impact on upstream and downstream industries, especially on the supply and demand relationship of expensive metals such as lithium, cobalt, and nickel. It is predicted that in the next few decades, lithium battery manufacturers will continue to maintain a high growth rate, while the supply of raw materials will face a long-term "supply exceeds demand" situation. Therefore, how to solve the problem of raw material supply in the lithium battery industry will become one of the keys to the healthy and stable development of the entire industry.

[0003] Considering that the service life of lithium batteries generally does not exceed 10 years, some commonly used digital product batteries are even difficult to exceed two years. Therefore, with the continuous development of social economy, the scrap volume of lithium-ion batteries will increase year by year. These scrapped lithium batteries contain a large amount of valuable metal resources, and their metal content is much higher than that of primary ore, and have a high recycling value. Among them, lithium resources are limited by uneven resource distribution and serious industry technical barriers, resulting in its output not keeping up with demand. At the same time, lithium carbonate extracted from lithium mines or lithium salt lakes often contains impurities such as sodium, potassium, magnesium and calcium, and often requires a lengthy impurity removal process to obtain battery-grade lithium carbonate sufficient to meet the production requirements of lithium batteries. Therefore, how to efficiently and quickly obtain high-purity lithium carbonate to meet the production requirements of lithium-ion battery manufacturers is of great strategic significance. At the same time, effectively recovering metal products from waste lithium-ion batteries that can be reused by lithium battery manufacturers can effectively alleviate the pressure on raw material supply and promote the healthy cycle development of the lithium battery industry, which has very important social significance.

[0004] Through searching the existing patent documents, it is found that CN 111613847 A discloses a method for efficiently recovering lithium from the positive electrode material of a lithium-ion battery, comprising the following steps: (1) pre-treating the positive electrode material of the lithium-ion battery to obtain a pre-treated positive electrode powder; (2) heating the pre-treated positive electrode powder with a reducing agent under the protection of an inert atmosphere to obtain a reduced positive electrode powder, wherein the reduced positive electrode powder contains an easily hydrolyzed lithium compound; (3) adding the reduced positive electrode powder to water for hydrolysis, and controlling the pH value of the hydrolysis system to 7-8, and the liquid-solid ratio to (2-3): 1; (4) after the hydrolysis is completed, the hydrolysis system in step (3) is subjected to solid-liquid separation, and the liquid phase is a lithium ion solution; adding soda ash to the lithium ion solution to obtain lithium carbonate. However, this method uses hydrogen as a reducing agent, which has a great explosion safety risk. In addition, this method also requires the configuration and construction of corresponding hydrogen production equipment, which increases the process cost and also increases the safety risk again. Therefore, it is of great practical significance to develop new, safe and easier-to-operate recovery methods to avoid the safety risks brought about by the use of hydrogen and reduce the operating costs of the process. Summary of the invention

[0005] The purpose of the present invention is to provide a method for recovering battery-grade lithium carbonate from positive electrode materials of lithium-ion batteries based on the complex types of lithium-ion batteries on the market, in view of the above problems; in particular, a method for recovering battery-grade lithium carbonate from positive electrode materials of lithium-transition metal oxide type lithium-ion batteries. The method is applicable to batteries of types such as lithium cobalt oxide, ternary lithium and lithium manganese oxide. First, the waste lithium-ion battery is discharged, and then separated by disassembly means to obtain positive electrode sheets; the positive electrode sheets are pyrolyzed to remove the binder, and the positive electrode materials are separated and enriched; the obtained positive electrode materials are reduced and converted by ammonia and then leached with water to obtain a lithium-rich aqueous solution; and the filtrate is heated, concentrated and chemically precipitated to recover battery-grade lithium carbonate. The present invention makes full use of the characteristics of single metal component and low impurity content in the positive electrode materials of lithium-ion batteries, and develops a method suitable for resource recovery of waste lithium-ion battery positive electrode materials. Compared with conventional recovery methods, it has the advantages of simple operation, low dosage of reagents and short process chain. The method recovers battery-grade lithium carbonate, which can be used for battery reproduction and manufacturing, and has great practical and social significance.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, the method comprising the following steps:

[0008] S1. Mix the waste lithium-ion battery positive electrode material and the ammonia producing agent in proportion, and place them in a reactor for oxygen-free calcination;

[0009] S2, the calcined product is leached with water and then filtered, the obtained filtrate is an aqueous solution rich in lithium ions, and the obtained filter residue is a transition metal element or oxide;

[0010] S3. After heating and concentrating the filtrate, add sodium carbonate precipitant and stir lightly to allow the metal ions to fully precipitate; filter and dry the precipitate to obtain battery-grade lithium carbonate.

[0011] As an embodiment of the present invention, in step S1, the lithium-ion battery is one or more types of lithium-transition metal oxide batteries.

[0012] As an embodiment of the present invention, the lithium-transition metal oxide type battery includes lithium cobalt oxide, ternary lithium, and lithium manganese oxide.

[0013] As an embodiment of the present invention, in step S1, the collection of waste lithium-ion battery positive electrode materials includes the following steps:

[0014] A1. Discharge the used lithium-ion battery until the residual voltage is less than 0.1V;

[0015] A2. Disassemble the discharged battery to obtain a positive electrode sheet, and perform pyrolysis on the obtained positive electrode sheet to remove the binder, and separate and collect the positive electrode material from the positive electrode sheet.

[0016] As an embodiment of the present invention, in step A1, the waste lithium-ion battery is discharged in a 0.5-2 mol / L sodium chloride solution.

[0017] As an embodiment of the present invention, in step A2, the reaction conditions of pyrolysis are 450-500° C. and vacuum calcination for 30-60 min.

[0018] In step S1, the positive electrode material is a positive electrode material separated and collected from a lithium-transition metal oxide type waste lithium ion battery, or a mixed material of positive electrode materials separated and collected from multiple lithium-transition metal oxide type waste lithium ion batteries.

[0019] As an embodiment of the present invention, in step S1, the ammonia generating agent is solid urea or melamine. The ammonia generating agent in this method is to produce ammonia gas without introducing strong acid, which only plays a reducing role; if other ammonium salts such as ammonium sulfate and ammonium bisulfate are used, the purpose of this application cannot be achieved.

[0020] As an embodiment of the present invention, in step S1, the oxygen-free calcination reaction conditions are: the ratio of the positive electrode material to the ammonia generating agent is 1:0.5-5 mol / mol, the filling rate of the reactor is 36-180 g / L, the reaction temperature is 500-600° C., and the reaction time is 10-40 min. The theoretical ammonia production in the ammonia generating agent can be converted into a mass ratio.

[0021] As an embodiment of the present invention, in step S2, the conditions for water leaching are: solid-liquid ratio of 10 g / L, filtration at room temperature, time of 30 min, and stirring speed of 200 rpm / min.

[0022] As an embodiment of the present invention, in step S3, heating and concentrating are performed until the volume is reduced by 10 to 20 times, a precipitant is added, the stirring speed is 200 rpm / min, and the sedimentation time is 20 min; and the filter residue is dried at 60° C. for more than 12 h (e.g., 12-24 h).

[0023] As an embodiment of the present invention, in step S3, the purity of the obtained lithium carbonate is greater than 99.9%.

[0024] Compared with the prior art, the method for recovering battery-grade lithium carbonate from a variety of waste lithium-ion batteries provided by the present invention has the following beneficial effects:

[0025] (1) It is suitable for processing a variety of lithium-transition metal oxide type lithium-ion batteries. It can process a single battery or mixed component batteries. It can effectively recover battery-grade lithium carbonate for the remanufacturing of positive electrode materials, thus realizing a closed-loop cycle of the industrial chain;

[0026] (2) In addition to lithium carbonate, high-purity transition metal elements or oxides can also be obtained, which can be used to prepare cathode material precursors and realize their resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0028] Figure 1 A process roadmap for a method of recovering battery-grade lithium carbonate from lithium-ion battery cathode materials;

[0029] Figure 2 X-ray diffraction (XRD) diagram of positive electrode materials obtained by disassembling and pyrolyzing different types of lithium-ion batteries in the present invention;

[0030] Figure 3 X-ray diffraction (XRD) diagrams of samples obtained after ammonia reduction roasting of different types of lithium ion battery positive electrode materials of the present invention;

[0031] Figure 4 The X-ray diffraction (XRD) diagram of the filter residue after water washing of the product of ammonia reduction roasting of different types of lithium ion battery positive electrode materials of the present invention;

[0032] Figure 5The figure is the X-ray diffraction (XRD) diagram of the battery-grade lithium carbonate recovered by the present invention. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0034] The reaction process of the present invention is as follows:

[0035] Ammonia production by decomposition of ammonia generating agent:

[0036] CO(NH2)2(s)+H2O(g)→CO2(g)+2NH3(g)

[0037] C3N6H6(s)+6H2O(g)→3CO2(g)+6NH3(g)

[0038] Ammonia reduction conversion of cathode materials:

[0039] 2LiCoO2(s)+2NH3(g)→2Co(s)+3H2O(g)+Li2O(s)+N2(g)

[0040] 2LiMn2O4(s)+2NH3(g)→4MnO(s)+3H2O(g)+Li2O(s)+N2(g)

[0041] 6LiNi x Co y Mn 1-x-y O2(s)+[4(x+y)+2]NH3(g)→6xNi(s)+6yCo(s)+6(1-xy))MnO(s)+[6(x+y)+3]H2O(g)+3Li2O(s)+[2(x+y)+1]N2(g)

[0042] Side effects:

[0043] Li2O(s)+CO2(g)→Li2CO3(s)

[0044] The separation and collection process of the positive electrode material in the following embodiments is as follows: the waste lithium-ion battery is discharged in a 1 mol / L sodium chloride solution until the residual voltage is less than 0.1 V; the discharged battery is disassembled to obtain a positive electrode sheet, and the obtained positive electrode sheet is pyrolyzed to remove the binder, and the positive electrode material is separated and collected from the positive electrode sheet.

[0045] Example 1

[0046] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0047] 1. Mix the waste lithium cobalt oxide battery positive electrode material and urea in a dosage ratio of 1:4 mol / mol as a reaction material for standby use, place the material in a ceramic crucible reactor, the added material and the reactor volume ratio is 72g / L, and keep the reaction at 550°C for 40min under a nitrogen atmosphere (flow rate 150mL / min);

[0048] 2. The solid after the roasting reaction was washed with water at room temperature at a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 99.23% and the selectivity was greater than 99.9%.

[0049] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0050] 4. Dry the filter residue at 60°C for 12 hours to obtain a high-purity cobalt solid product.

[0051] Example 2

[0052] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0053] 1. The waste lithium manganese oxide battery positive electrode material and urea were mixed in a dosage ratio of 1:4 mol / mol as a reaction material for standby use, and the materials were placed in a ceramic crucible reactor with a ratio of 36 g / L of the added material to the reactor content. The reaction was carried out at 600°C for 30 min under a nitrogen atmosphere (flow rate 150 mL / min);

[0054] 2. The solid after the roasting reaction was washed with water at room temperature according to a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 99.11% and the selectivity was greater than 99.5%.

[0055] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0056] 4. Dry the filter residue at 60°C for 12 h to obtain a high-purity manganese monoxide product.

[0057] Example 3

[0058] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0059] 1. Mix the waste ternary lithium battery positive electrode material and melamine in a ratio of 1:0.55 mol / mol (mass ratio is about 1:0.7 w / w) as a reaction material for standby use, place the material in a ceramic crucible reactor, the added material and the reactor volume ratio is 108 g / L, and react at 600 ° C for 20 min under a nitrogen atmosphere (flow rate 150 mL / min);

[0060] 2. The solid after the roasting reaction was washed with water at room temperature according to a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 99.90% and the selectivity was greater than 99.8%.

[0061] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0062] 4. Dry the filter residue at 60°C for 12 hours to obtain a mixed product of cobalt / nickel elements and manganese monoxide.

[0063] Example 4

[0064] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0065] 1. Mix the waste lithium cobalt oxide battery positive electrode material and urea in a dosage ratio of 1:4 mol / mol as a reaction material for standby use, place the material in a ceramic crucible reactor, the added material and the reactor volume ratio is 36g / L, and react at 500°C for 30min under a nitrogen atmosphere (flow rate 150mL / min);

[0066] 2. The solid after the roasting reaction was washed with water at room temperature according to a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 76.52% and the selectivity was greater than 99.7%.

[0067] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0068] 4. Dry the filter residue at 60°C for 12 hours to obtain a mixed product of cobalt element and partial lithium cobaltate residue.

[0069] Example 5

[0070] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0071] 1. Mix the waste lithium cobalt oxide battery positive electrode material and urea in a dosage ratio of 1:4 mol / mol as a reaction material for standby use, place the material in a ceramic crucible reactor, the added material and the reactor volume ratio is 36g / L, and keep the reaction at 550°C for 5min under a nitrogen atmosphere (flow rate 150mL / min);

[0072] 2. The solid after the roasting reaction was washed with water at room temperature according to a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 86.25% and the selectivity was greater than 99.97%.

[0073] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0074] 4. Dry the filter residue at 60°C for 12 hours to obtain a mixed product of cobalt element and partial lithium cobaltate residue.

[0075] Example 6

[0076] This embodiment relates to a method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, such as Figure 1 , including the following steps:

[0077] 1. Mix the waste ternary lithium battery positive electrode material and melamine in a dosage ratio of 1:1 mol / mol as a reaction material for standby use, place the material in a ceramic crucible reactor, the added material and the reactor volume ratio is 72g / L, and keep the reaction at 550°C for 30min under a nitrogen atmosphere (flow rate 150mL / min);

[0078] 2. The solid after the roasting reaction was washed with water at room temperature according to a solid-liquid ratio of 10 g / L, and filtered to obtain a lithium-containing aqueous solution and a cobalt elemental filter residue, respectively. The lithium leaching rate was 99.71% and the selectivity was greater than 99.99%.

[0079] 3. Heat the lithium-containing aqueous solution to 70-80°C and concentrate until the volume is reduced by 10 times, slowly add 2 mol / L sodium carbonate solution (stirring at 200 rpm / min) until there is no obvious increase in precipitation, the sedimentation time is 20 min, filter the precipitate and dry it at 60°C for 12 h to obtain battery-grade lithium carbonate;

[0080] 4. Dry the filter residue at 60°C for 12 hours to obtain a mixed product of cobalt / nickel elements and manganese monoxide.

[0081] Figure 2 The X-ray diffraction (XRD) diagram of the positive electrode material (corresponding to Examples 1, 2, and 3) obtained by disassembling and pyrolyzing different types of lithium-ion batteries of the present invention is shown in FIG. Figure 2 It can be seen that the positive electrode material can be effectively obtained through "discharge-disassembly-pyrolysis" to prepare for the next reaction;

[0082] Figure 3 The X-ray diffraction (XRD) diagrams of samples obtained after ammonia reduction roasting of different types of lithium ion battery positive electrode materials of the present invention are shown in FIG. Figure 3 It can be seen that three different types of positive electrode materials, lithium cobalt oxide, lithium manganese oxide and ternary lithium, can be effectively converted into water-soluble lithium carbonate and water-insoluble metal elements or metal oxides after ammonia reduction and roasting;

[0083] Figure 4 The X-ray diffraction (XRD) diagram of the filter residue after water washing of the product of ammonia reduction roasting of different types of lithium ion battery positive electrode materials of the present invention is shown in FIG. Figure 4 It can be seen that after the products of three different types of positive electrode materials, lithium cobalt oxide, lithium manganese oxide and ternary lithium, are reduced and calcined with ammonia, the lithium carbonate dissolved in water can be selectively extracted after a simple water washing operation, while the transition metal remains intact;

[0084] Figure 5 The X-ray diffraction (XRD) diagram of the battery-grade lithium carbonate recovered in Example 1 of the present invention is shown in FIG. Figure 5 It can be seen that the lithium-containing aqueous solution extracted after washing can be subjected to a chemical precipitation operation to obtain battery-pure lithium carbonate powder. Since the present invention selectively extracts Li, the selectivity is close to 100%, that is, the lithium-containing solution obtained by the method of the present invention (including all embodiments) contains almost only Li and no other metals, so when a chemical precipitation operation is adopted, the obtained lithium carbonate reaches battery-grade purity.

[0085] In summary, the present invention uses an ammonia reduction roasting method to achieve selective recovery of lithium resources in positive electrode materials, reducing the large-scale use of reducing agents such as strong acids, while also recovering high-purity transition metal elements or oxides, thereby achieving effective recovery of metal resources in positive electrode materials. This method uses an ammonia reduction conversion process widely used in industry, uses less chemical agents, and achieves recovery of battery-grade lithium carbonate, which has broad industrial application potential.

[0086] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material, characterized in that: The method comprises the following steps: S1. Mix the cathode material of waste lithium-ion battery and the ammonia producing agent in proportion, and place them in a reactor for anaerobic roasting treatment; the lithium-ion battery is one or more of lithium-transition metal oxide type batteries, and the lithium-transition metal oxide type battery is lithium cobalt oxide, ternary lithium or lithium manganese oxide; the ammonia producing agent is solid urea or melamine; the anaerobic roasting reaction conditions are: the amount ratio of the cathode material to the ammonia producing agent is 1:0.5-5 mol / mol, the filling rate of the reactor is 36-180 g / L, the reaction temperature is 550-600°C, and the reaction time is 10-40 min; The reaction process is as follows: Ammonia production by decomposition of ammonia generating agent: CO(NH2)2(s)+H2O(g)→CO2(g)+2NH3(g), Or, C3N6H6(s)+6H2O(g)→3CO2(g)+6NH3(g); Ammonia reduction conversion of cathode materials: 2LiCoO2(s)+2NH3(g)→2Co(s)+3H2O(g)+Li2O(s)+N2(g), Or, 2LiMn2O4(s)+2NH3(g)→4MnO(s)+3H2O(g)+Li2O(s)+N2(g), Or, 6LiNi x Co y Mn 1-x-y O2(s) + [4(x + y) + 2]NH3(g) → 6xNi(s) + 6yCo(s) + 6(1 - x - y))MnO(s) + [6(x + y) + 3]H2O(g) + 3Li2O(s) + [2(x + y) + 1]N2(g); Side effects: Li2O(s)+CO2(g)→Li2CO3(s); S2. The calcined product is leached with water and then filtered. The obtained filtrate is an aqueous solution rich in lithium ions, and the obtained filter residue is a transition metal element or oxide. The leaching rate of lithium after leaching is above 99.11%, and the selectivity is greater than 99.5%; S3. After heating and concentrating the filtrate, add sodium carbonate precipitant and stir lightly to allow the metal ions to fully precipitate; filter and dry the precipitate to obtain battery-grade lithium carbonate.

2. The method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material according to claim 1, characterized in that: In step S1, the collection of waste lithium-ion battery positive electrode materials includes the following steps: A1. Discharge the used lithium-ion battery until the residual voltage is less than 0.1V; A2. Disassemble the discharged battery to obtain a positive electrode sheet, and perform pyrolysis on the obtained positive electrode sheet to remove the binder, and separate and collect the positive electrode material from the positive electrode sheet.

3. The method for recovering battery-grade lithium carbonate from a lithium-ion battery cathode material according to claim 2, wherein: In step A1, the waste lithium-ion battery is discharged in a 0.5-2 mol / L sodium chloride solution.

4. The method for recovering battery-grade lithium carbonate from a lithium-ion battery cathode material according to claim 2, wherein: In step A2, the reaction conditions of pyrolysis are 450-500° C. and vacuum calcination for 30-60 min.

5. The method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material according to claim 1, characterized in that: In step S3, the mixture is heated and concentrated until the volume is reduced by 10 to 20 times, a precipitant is added, the stirring speed is 200 rpm / min, and the sedimentation time is 20 min; and the filter residue is dried at 60° C. for more than 12 h.

6. The method for recovering battery-grade lithium carbonate from a lithium-ion battery positive electrode material according to claim 1, characterized in that: In step S3, the purity of the obtained lithium carbonate is greater than 99.9%.