A tower surface protective composite material and its preparation method and application

Through the combination of aluminized Al2O3 fiber composite aluminum alloy coating and organic anti-corrosion layer, an efficient protective layer is formed, which solves the problem of insufficient protection of tower surface protection composite materials in extreme environments, significantly improves the corrosion resistance and protection period, and meets the requirements of wind power Tower protection requirements.

CN114277331BActive Publication Date: 2024-10-01HUADIAN HEAVY MACHINERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111632645.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-10-01
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

Existing tower surface protection composite materials are insufficiently protected in extreme environments and cannot meet the effects of high and low temperatures, wind, sand, wind and rain, etc., resulting in insufficient protection periods and serious problems of vibration fatigue and corrosion damage.

Method used

Using a combined preparation method of aluminized Al2O3 fiber composite aluminum alloy coating, high-build epoxy paint and polyurethane topcoat, a 30 μm-90 μm aluminized Al2O3 fiber composite aluminum alloy coating is formed by spraying and shot blasting, and on it Apply high-build epoxy paint and polyurethane topcoat in sequence to form an efficient protective layer.

Benefits of technology

It significantly improves the corrosion resistance of the tower in the wind and sand blowing environment, extends the protection period, meets the protection needs of the wind power tower, and the adhesion and salt spray resistance meet the index requirements of the wind power tower.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114277331B_ABST
    Figure CN114277331B_ABST
Patent Text Reader

Abstract

The present invention discloses a tower surface protection composite material and its preparation method and application. The present invention forms a tower surface protection composite material composed of an aluminum-plated Al2O3 fiber composite aluminum alloy coating and sequentially coated with thick paste type epoxy paint and polyurethane topcoat on the surface of the tower substrate through the preparation of aluminum-plated aluminum oxide fiber, the preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire, tower substrate coating treatment, aluminum-plated Al2O3 fiber composite aluminum alloy coating strengthening treatment and organic anti-corrosion layer. The thickness of the aluminum-plated Al2O3 fiber composite aluminum alloy coating is 30μm-90μm, the dry film thickness of the thick paste type epoxy paint is not less than 120μm, and the dry film thickness of the polyurethane topcoat is not less than 40μm. The tower surface protection composite material prepared by the present invention is suitable for large-scale industrial production, can improve the corrosion resistance of the tower in a wind and sand erosion environment, and can be used for the surface protection of wind power towers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and in particular relates to a tower surface protective composite material and a preparation method and application thereof. Background Art

[0002] With the continuous consumption of traditional energy reserves and the increasingly serious environmental problems caused by its use, the development and utilization of clean energy has become an important theme and content of the development of the world today. Wind energy is an important green energy source with the advantages of being renewable, clean and pollution-free, and widely distributed, and has broad prospects for development and application. As the supporting foundation and operating platform of the wind turbine system, the wind turbine tower is an important guarantee for the safe operation of the wind turbine system. In actual engineering applications, vibration fatigue fracture and corrosion damage are the main forms of failure of wind turbine towers, and corrosion damage will further cause and aggravate the occurrence of vibration fatigue fracture. Therefore, anti-corrosion treatment is the focus of attention in the field of tower manufacturing.

[0003] The existing outer surface of the tower is usually treated in the following way: in a medium-corrosive environment, a thick paste epoxy paint is used as the base layer, and a polyurethane topcoat is used as the surface layer. When long-term protection is required, the thickness of the base layer is increased; in a high-corrosive environment, an epoxy zinc-rich primer is used as the base layer, an epoxy micaceous iron intermediate paint is used as the middle layer, and a polyurethane topcoat is used as the surface layer. When long-term protection is required, the thickness of the middle layer is increased. As the environment of the application scenarios becomes increasingly complex, the impact of factors such as high and low temperatures, wind and sand, wind and rain, and light on wind turbine towers is becoming increasingly prominent, and the shortcomings of pure organic protective composite materials in extreme environments are becoming more and more obvious. It is of great significance to improve the protection period of the protective composite materials on the tower while improving the stability of the protective composite materials themselves. Summary of the invention

[0004] The purpose of the present invention is to provide a tower surface protection composite material and a preparation method and application thereof.

[0005] First, according to one aspect of the present invention, the present invention provides a method for preparing a tower surface protective composite material, the preparation method comprising the following steps:

[0006] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0007] 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 2.0%-5.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200nm and the length is 600nm;

[0008] 2) Preparation of composite alloy melt: melting an aluminum ingot at 770°C, adding various master alloys, maintaining the temperature at 750°C and performing electromagnetic stirring for 20 minutes, standing for 30 minutes, refining, degassing, deslagging and heating to 770°C to obtain an aluminum alloy melt; adding aluminum-plated Al2O3 fibers with a weight ratio of 2.0% to 5.0% to the aluminum alloy melt, electromagnetically stirring at 750°C for 30 minutes, standing for 10 minutes, and obtaining a composite alloy melt;

[0009] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 15%-20%; drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ0.5mm-Φ1.5mm by multiple drawing processes;

[0010] 2. Tower Base Coating Treatment

[0011] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0012] 2) Spraying treatment: a high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 10m / min-15m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 30μm-90μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0013] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0014] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base is strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm are selected, the shot peening pressure is 0.2-0.5 MPa, and the shot peening distance is 250 mm, so as to obtain the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment.

[0015] 4. Preparation of organic anticorrosive layer

[0016] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0017] The present invention also relates to the application of the method for preparing the tower surface protective composite material in the field of tower anti-corrosion material preparation.

[0018] According to another aspect of the present invention, the present invention provides a tower surface protective composite material prepared according to the above preparation method.

[0019] Furthermore, the tower surface protection composite material involved in the present invention consists of an aluminum-plated Al2O3 fiber composite aluminum alloy coating layer and a thick paste type epoxy paint and a polyurethane topcoat coated in sequence.

[0020] Furthermore, in the tower surface protection composite material of the present invention, the thickness of the aluminum-plated Al2O3 fiber composite aluminum alloy coating is 30μm-90μm.

[0021] Furthermore, in the tower surface protection composite material of the present invention, the dry film thickness of the high build-up epoxy paint is not less than 120 μm.

[0022] Furthermore, in the tower surface protection composite material of the present invention, the dry film thickness of the polyurethane topcoat is not less than 40 μm.

[0023] Finally, the present invention also relates to the application of the above tower surface protection composite material in the field of tower corrosion protection.

[0024] Compared with the prior art, the preparation method of the tower surface protection composite material of the present invention is suitable for large-scale industrial production, can improve the corrosion resistance of the tower in a wind and sand erosion environment, and can be used for the surface protection of wind power towers. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0026] Figure 1 This is a corrosion morphology of the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment of the sample prepared in Example 3;

[0027] Figure 2 This is the corrosion morphology of the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment of the sample prepared in Example 5. DETAILED DESCRIPTION

[0028] The following describes in detail the embodiments of the present invention through specific examples, but the following specific embodiments are essentially examples. The present invention can also be implemented or applied through other different specific embodiments. The details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0029] Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, any methods, equipment, and materials of the prior art that are similar or equivalent to the methods, equipment, and materials in the embodiments of the present invention may be used to implement the present invention, based on the prior art mastery of those skilled in the art and the description of the present invention.

[0030] Example 1

[0031] A method for preparing a tower surface protective composite material:

[0032] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0033] 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 2.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200 nm and the length is 600 nm;

[0034] 2) Preparation of composite alloy melt: melt the aluminum ingot at 770°C, add various master alloys, keep the temperature at 750°C and perform electromagnetic stirring for 20 minutes, let it stand for 30 minutes, refine, degas, remove slag and heat to 770°C to obtain an aluminum alloy melt; add 2.0% by weight of aluminum-plated Al2O3 fiber to the aluminum alloy melt, stir it electromagnetically at 750°C for 30 minutes, let it stand for 10 minutes to obtain a composite alloy melt;

[0035] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 20%; and drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ0.5 mm by multiple drawing processes;

[0036] 2. Tower Base Coating Treatment

[0037] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0038] 2) Spraying treatment: A high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 15m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 30μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0039] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0040] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base was strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm were selected, the shot peening pressure was 0.2 MPa, and the shot peening distance was 250 mm. The aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment was obtained.

[0041] 4. Preparation of organic anticorrosive layer

[0042] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0043] Example 2

[0044] A method for preparing a tower surface protective composite material:

[0045] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0046] 1) Ingredients: The following ingredients are prepared by weight percentage: 0.22% iron Fe, 0.09% silicon Si, 0.05% copper Cu, 0.002% magnesium Mg, 0.02% nickel Ni, 0.002% neodymium Nd, 3.0% aluminum-plated Al2O3 fiber, and the balance is aluminum Al, to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fiber is 200nm and the length is 600nm;

[0047] 2) Preparation of composite alloy melt: melt the aluminum ingot at 770°C, add various master alloys, keep the temperature at 750°C and perform electromagnetic stirring for 20 minutes, let it stand for 30 minutes, refine, degas, remove slag and heat to 770°C to obtain an aluminum alloy melt; add aluminum-plated Al2O3 fibers with a weight ratio of 3.0% to the aluminum alloy melt, stir them electromagnetically at 750°C for 30 minutes, let it stand for 10 minutes to obtain a composite alloy melt;

[0048] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 20%; and drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ0.8 mm by multiple drawing processes;

[0049] 2. Tower Base Coating Treatment

[0050] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0051] 2) Spraying treatment: a high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 12m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 50μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0052] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0053] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base was strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm were selected, the shot peening pressure was 0.2 MPa, and the shot peening distance was 250 mm. The aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment was obtained.

[0054] 4. Preparation of organic anticorrosive layer

[0055] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0056] Example 3

[0057] A method for preparing a tower surface protective composite material:

[0058] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0059] 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 4.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200 nm and the length is 600 nm;

[0060] 2) Preparation of composite alloy melt: melt the aluminum ingot at 770°C, add various master alloys, keep the temperature at 750°C and perform electromagnetic stirring for 20 minutes, let it stand for 30 minutes, refine, degas, remove slag and heat to 770°C to obtain an aluminum alloy melt; add aluminum-plated Al2O3 fibers with a weight ratio of 4.0% to the aluminum alloy melt, stir them electromagnetically at 750°C for 30 minutes, let it stand for 10 minutes to obtain a composite alloy melt;

[0061] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 18%; and drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ1.0 mm by multiple drawing processes;

[0062] 2. Tower Base Coating Treatment

[0063] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0064] 2) Spraying treatment: A high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 13m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 60μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0065] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0066] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base was strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm were selected, the shot peening pressure was 0.3 MPa, and the shot peening distance was 250 mm. The aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment was obtained.

[0067] 4. Preparation of organic anticorrosive layer

[0068] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0069] Example 4

[0070] A method for preparing a tower surface protective composite material:

[0071] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0072] 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 4.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200 nm and the length is 600 nm;

[0073] 2) Preparation of composite alloy melt: melt the aluminum ingot at 770°C, add various master alloys, keep the temperature at 750°C and perform electromagnetic stirring for 20 minutes, let it stand for 30 minutes, refine, degas, remove slag and heat to 770°C to obtain an aluminum alloy melt; add aluminum-plated Al2O3 fibers with a weight ratio of 4.0% to the aluminum alloy melt, stir them electromagnetically at 750°C for 30 minutes, let it stand for 10 minutes to obtain a composite alloy melt;

[0074] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 15%; and drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ1.2 mm by multiple drawing processes;

[0075] 2. Tower Base Coating Treatment

[0076] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0077] 2) Spraying treatment: a high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 10m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 90μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0078] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0079] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base was strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm were selected, the shot peening pressure was 0.5 MPa, and the shot peening distance was 250 mm, and the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment was obtained.

[0080] 4. Preparation of organic anticorrosive layer

[0081] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0082] Example 5

[0083] A method for preparing a tower surface protective composite material:

[0084] 1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire

[0085] 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 5.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200 nm and the length is 600 nm;

[0086] 2) Preparation of composite alloy melt: melt the aluminum ingot at 770°C, add various master alloys, keep the temperature at 750°C and perform electromagnetic stirring for 20 minutes, let it stand for 30 minutes, refine, degas, remove slag and heat to 770°C to obtain an aluminum alloy melt; add aluminum-plated Al2O3 fibers with a weight ratio of 5.0% to the aluminum alloy melt, stir them electromagnetically at 750°C for 30 minutes, let it stand for 10 minutes to obtain a composite alloy melt;

[0087] 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 15%; drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ1.5 mm by multiple drawing processes;

[0088] 2. Tower Base Coating Treatment

[0089] 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment;

[0090] 2) Spraying treatment: a high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 10m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 90μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

[0091] 3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating

[0092] The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base was strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm were selected, the shot peening pressure was 0.5 MPa, and the shot peening distance was 250 mm, and the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment was obtained.

[0093] 4. Preparation of organic anticorrosive layer

[0094] A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

[0095] Example 6

[0096] According to the salt spray test method of GB / T 10125 "Artificial atmosphere corrosion test-salt spray test", the Al2O3 fiber composite aluminum alloy coating obtained in Examples 1 to 5 after strengthening treatment was subjected to salt spray corrosion test. The test time was 30 days, the spray mode was continuous, the test temperature was 35±2℃, and the salt spray deposition rate was 1-2ml·80cm -2 ·h -1 The salt spray corrosion solution is a sodium chloride solution with a concentration of 50g / l±5g / l, and the pH value of the sodium chloride solution is 7.0. The weight change of each sample is calculated by weighing method, and the test results are shown in Table 1.

[0097] Table 1

[0098]

[0099] The corrosion morphology of the samples prepared in Example 3 and Example 5 was observed using a scanning electron microscope of model JSM-6490LV. Figure 1 As shown, after 30 days of salt spray corrosion, the sample prepared in Example 3 has white corrosion products on the surface of the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment. Except for local accumulation, the overall particle size of the corrosion products is small. Figure 2 As shown, compared with Example 3, after 30 days of salt spray corrosion, the white corrosion product particles on the surface of the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment are significantly larger and appear as local clusters in multiple regions. This is consistent with the test results measured by the weighing method.

[0100] According to the cross-cut test in the adhesion performance test method in GB / T 9793 "Thermal spraying metal and other inorganic coatings of zinc, aluminum and their alloys", the aluminum-plated Al2O3 fiber composite aluminum alloy coatings prepared in Examples 1 to 5 were tested for adhesion. When the cross-cut area was 15 mm×15 mm and the scratch spacing was 3 mm, an adhesive tape was used to press the coating in the cross-cut area with a load of 5N and quickly pulled apart in a direction perpendicular to the surface of the coating, and the coating did not peel off or crack.

[0101] According to the wind turbine tower surface protection layer detection index requirements, the performance of the thick paste epoxy paint and polyurethane topcoat in the tower surface protection composite materials prepared in Examples 1 to 5 was tested. The test results are shown in Tables 2 and 3.

[0102] Table 2

[0103]

[0104] Table 3

[0105]

[0106] It can be seen from Table 1 that the adhesion, salt spray resistance and flexibility of the tower surface protection composite materials prepared in Examples 1 to 5 meet the index requirements for wind power tower protection.

[0107] The above-described embodiments of the present invention do not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a tower surface protective composite material, characterized in that: The preparation method comprises the following steps:

1. Preparation of Aluminum-coated Al2O3 Fiber Composite Aluminum Alloy Wire 1) Ingredients: The following ingredients are prepared by weight percentage: iron Fe 0.22%, silicon Si 0.09%, copper Cu 0.05%, magnesium Mg 0.002%, nickel Ni 0.02%, neodymium Nd 0.002%, aluminum-plated Al2O3 fiber 2.0%-5.0%, and the balance is aluminum Al, so as to prepare aluminum ingots, aluminum master alloys and aluminum-plated Al2O3 fibers; wherein the diameter of the aluminum-plated Al2O3 fibers is 200nm and the length is 600nm; 2) Preparation of composite alloy melt: melting an aluminum ingot at 770°C, adding various master alloys, maintaining the temperature at 750°C and performing electromagnetic stirring for 20 minutes, standing for 30 minutes, refining, degassing, deslagging and heating to 770°C to obtain an aluminum alloy melt; adding aluminum-plated Al2O3 fibers with a weight ratio of 2.0% to 5.0% to the aluminum alloy melt, electromagnetically stirring at 750°C for 30 minutes, standing for 10 minutes, and obtaining a composite alloy melt; 3) Preparation of aluminum-plated Al2O3 fiber composite aluminum alloy wire: forming the composite alloy melt into an aluminum alloy rod blank by hot extrusion, wherein the hot extrusion temperature is 640°C-650°C and the extrusion area reduction ratio is 15%-20%; drawing the aluminum alloy rod blank into an aluminum-plated Al2O3 fiber composite aluminum alloy wire with a specification of Φ0.5mm-Φ1.5mm by multiple drawing processes; 2. Tower Base Coating Treatment 1) Surface treatment of the tower base: Use 1mm quartz sand to perform mechanical sandblasting on the surface of the tower base, the sandblasting pressure is 2.0MPa, and the sandblasting distance is 300mm; use acetone to remove oil, 0.05mol / L dilute hydrochloric acid to remove rust, rinse with deionized water, and dry to obtain the tower base after surface treatment; 2) Spraying treatment: a high-speed spray gun is used to spray the aluminum-plated Al2O3 fiber composite aluminum alloy wire on the surface of the tower base after surface treatment. The spraying temperature is 820°C, the spraying air pressure is 1.5MPa, the oxygen pressure is 0.55MPa, and the acetylene pressure is 0.05MPa. The wire feeding speed of the aluminum-plated Al2O3 fiber composite aluminum alloy wire is 10m / min-15m / min, the spraying distance is 200mm, and the spraying angle is 25°, forming a 30μm-90μm aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base.

3. Strengthening treatment of aluminum-plated Al2O3 fiber composite aluminum alloy coating The aluminum-plated Al2O3 fiber composite aluminum alloy coating on the surface of the tower base is strengthened by using a dry shot peening machine. Zirconia ceramic shots with an average particle size of 0.5 mm are selected, the shot peening pressure is 0.2-0.5 MPa, and the shot peening distance is 250 mm, so as to obtain the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment.

4. Preparation of organic anticorrosive layer A thick build epoxy paint and a polyurethane topcoat are sequentially applied on the aluminum-plated Al2O3 fiber composite aluminum alloy coating after strengthening treatment, the dry film thickness of the thick build epoxy paint is not less than 120 μm, and the dry film thickness of the polyurethane topcoat is not less than 40 μm, to obtain a tower surface protective composite material.

2. Application of the preparation method of the tower surface protective composite material according to claim 1 in the field of tower anti-corrosion material preparation.

3. A tower surface protective composite material, characterized in that: The tower surface protective composite material is prepared according to the preparation method according to claim 1.

4. The tower surface protective composite material according to claim 3, characterized in that: The tower surface protection composite material consists of an aluminum-plated Al2O3 fiber composite aluminum alloy coating layer and a thick paste type epoxy paint and a polyurethane topcoat coated in sequence.

5. The tower surface protective composite material according to claim 4, characterized in that: The thickness of the aluminum-plated Al2O3 fiber composite aluminum alloy coating is 30 μm-90 μm.

6. The tower surface protective composite material according to claim 5, characterized in that: The dry film thickness of the high build epoxy paint is not less than 120 μm.

7. The tower surface protective composite material according to claim 6, characterized in that: The dry film thickness of the polyurethane topcoat is not less than 40 μm.

8. Application of the tower surface protection composite material according to any one of claims 3 to 7 in the field of tower corrosion protection.