A lithium metal processing method and application thereof

The solid electrolyte interface layer is formed through amide solution treatment, which solves the problem of poor stability of metal lithium anode materials in lithium batteries, significantly improves the rate performance and calendar life of lithium batteries, and achieves higher battery storage stability and service life.

CN114293185BActive Publication Date: 2024-11-08EVE ENERGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111636343.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2024-11-08
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

Metal lithium anode materials have problems such as poor rate discharge performance, poor stability and short calendar life in lithium batteries, which affect the application performance of lithium batteries.

Method used

The metal lithium is treated with amide solution to form a dense solid electrolyte interface layer to protect the surface of the metal lithium and improve its stability and battery performance.

Benefits of technology

Through amide treatment, the calendar life and rate discharge performance of lithium batteries are significantly improved, ensuring the battery's capacity retention rate and internal resistance change rate under high temperature environments, and improving the battery's storage stability and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a lithium metal treatment method and application thereof, the method comprising the following steps: (1) mixing an amide and an organic solvent to obtain an amide solution; (2) coating the amide solution on the surface of metallic lithium to obtain treated metallic lithium. The present invention pre-coats the metallic lithium with amide to form a protective layer to protect the metallic lithium, thereby improving the stability of the metallic lithium as an active material, and further improving the calendar life and rate discharge performance of the lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative electrode materials and relates to a lithium metal processing method and application thereof. Background Art

[0002] Due to their excellent performance, lithium primary batteries are widely used in cameras, watches, electronic security, memory backup power supplies, laptop backup power supplies and other fields.

[0003] Metallic lithium has a low electrochemical potential (-3.045V vs. standard hydrogen electrode) and is widely used as anode material for primary batteries (such as lithium-sulfur batteries, lithium-air batteries, lithium-thionyl chloride batteries, lithium-manganese dioxide batteries, lithium-carbon fluoride batteries, etc.). However, the negative electrode of metallic lithium has high reduction activity and poor stability, which causes the side reactions between the negative electrode active material and the electrolyte to gradually increase during the storage of lithium batteries, resulting in a decrease in active materials, a gradual thickening of the solid electrolyte interface film, and an increase in internal resistance, which ultimately deteriorates the battery capacity, reduces the battery calendar life and rate performance.

[0004] CN102623670A discloses a metal lithium primary battery negative electrode sheet, involving a battery structure, comprising a sheet-like body, a strip metal and a negative electrode tab; firstly, the strip metal is placed on the sheet-like body to press them together, and then the negative electrode tab is pressed and inlaid with the sheet-like body to form a whole; the sheet-like body is a metal lithium foil or a lithium aluminum alloy foil; the strip metal is a metal mesh or a metal foil; its material is any one of copper mesh, copper foil, aluminum mesh, aluminum foil, nickel mesh, nickel foil, steel mesh, and steel foil; the negative electrode tab is pure nickel with hot melt adhesive attached to the nickel strip, and the lithium metal negative electrode sheet has poor rate discharge performance and poor stability.

[0005] CN111952571A discloses a lithium / lithium alloy composite negative electrode for high-power primary batteries, a preparation method and a battery, wherein the lithium is a metal lithium foil, the lithium alloy is a lithium alloy powder, and the composite negative electrode comprises: two layers of metal lithium foil and a lithium alloy as an intermediate layer; the lithium alloy is arranged between the two layers of the metal lithium foil; the composite negative electrode is obtained by rolling the metal lithium foil and the lithium alloy together. The calendar life of the lithium / lithium alloy composite negative electrode is relatively short, which affects its application in lithium primary batteries.

[0006] The lithium negative electrode plate described in the above scheme has the problems of poor rate discharge performance, poor stability or short calendar life. Therefore, it is very necessary to develop a metal lithium treatment method to improve the rate discharge performance, calendar life and stability of the metal lithium negative electrode. Summary of the invention

[0007] The purpose of the present invention is to provide a lithium metal treatment method and application thereof. The present invention pre-coats lithium metal with amide treatment, and uses an amide solution to treat the lithium metal. The unique carbonyl group (C=O) in the amide group is conjugated with the electrons on the nitrogen atom (N), which reduces the NH bond electron cloud density, so that the surface of the amide metal lithium negative electrode exhibits higher chemical activity, and can quickly form a dense protective layer on the surface of the lithium metal to protect the lithium metal, thereby improving the stability of the lithium metal as an active material, and further improving the calendar life and rate discharge performance of the lithium battery.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for treating lithium metal, the method comprising the following steps:

[0010] (1) mixing an amide and an organic solvent to obtain an amide solution;

[0011] (2) coating the amide solution on the surface of metallic lithium to obtain treated metallic lithium.

[0012] The present invention aims at the instability of metallic lithium. Before the metallic lithium is used, it is immersed in an amide treatment solution or sprayed on the surface of the metallic lithium. The amide can react with the metallic lithium to pre-form a layer of artificial interface on the surface of the metallic lithium, thereby protecting the metallic lithium negative electrode and improving the storage stability, service life and rate performance of the battery.

[0013] The present invention uses an amide-based metal lithium negative electrode treatment solution to generate a dense solid electrolyte interface layer rich in nitrogen compounds (such as LiN(R)2, Li2NR, Li3N, etc.) and LiOH, Li2CO3, etc. on the surface of the metal lithium. The interface layer has high ionic conductivity and significantly isolates the contact between the active components of the electrolyte and the active metal lithium, thereby improving the high-power discharge performance and calendar life of the battery.

[0014] Preferably, the amide in step (1) comprises any one of carbonyl amide, alkyl amide or halogenated amide, or a combination of at least two thereof.

[0015] The present invention uses an amide solution to treat metallic lithium. Compared with amines, the unique carbonyl group (C=O) in the amide group is conjugated with electrons on the nitrogen atom (N), which reduces the NH bond electron cloud density, so that the surface of the amide metal lithium negative electrode exhibits higher chemical activity, and can quickly form a dense and stable solid electrolyte interface layer on the surface of the metallic lithium, blocking the physical contact between fresh metallic lithium and solution components, thereby improving the stability of the metallic lithium.

[0016] Preferably, the organic solvent in step (1) comprises any one of carbonates, carboxylates, ethers, nitriles or carbon disulfide, or a combination of at least two thereof.

[0017] Preferably, the organic solvent comprises any one of dimethyl carbonate, ethyl methyl carbonate, propyl carbonate, fluoroethylene carbonate, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, ether, tetrahydrofuran, ethylene glycol dimethyl ether, fluoroether, 1,3-dioxolane, acetonitrile, propionitrile, butyronitrile, adiponitrile, succinonitrile or carbon disulfide, or a combination of at least two thereof.

[0018] Preferably, based on the mass of the amide solution being 100%, the mass fraction of the amide is 2-10%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0019] In the metal lithium treatment method described in the present invention, the mass concentration of amide in the amide solution will affect the treatment effect of the metal lithium. When the mass concentration of amide in the amide solution is controlled at 2-10%, the treatment effect of the metal lithium is better. If the mass concentration of amide is too low, the capacity retention rate (calendar life) after high-temperature storage is low, and the internal resistance change rate is large. If the mass concentration of amide is too high, the capacity retention rate and internal resistance change rate after battery storage are not further improved.

[0020] Preferably, the coating method in step (2) includes spraying and / or dipping.

[0021] Preferably, the coating time in step (2) is 5 to 60 minutes, for example, 5 minutes, 10 minutes, 20 minutes, 30 minutes or 60 minutes.

[0022] Preferably, the coating humidity is ≤150 ppm, for example: 5 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm, 100 ppm or 150 ppm, etc., preferably ≤50 ppm.

[0023] Preferably, the metallic lithium in step (2) comprises lithium sheets and / or lithium strips.

[0024] In a second aspect, the present invention provides a metallic lithium negative electrode material, which is prepared by the lithium metal processing method as described in the first aspect.

[0025] The surface of the metal lithium negative electrode material of the present invention has a dense and stable solid electrolyte interface layer, which blocks the physical contact between the metal lithium and the solution components and plays a role in improving the stability of the metal lithium.

[0026] In a third aspect, the present invention provides a negative electrode plate, wherein the negative electrode plate comprises the metallic lithium negative electrode material as described in the second aspect.

[0027] In a fourth aspect, the present invention provides a lithium primary battery, wherein the lithium primary battery comprises the negative electrode sheet as described in the third aspect.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention aims at the instability of metallic lithium. Before the metallic lithium is used, it is immersed in an amide treatment solution or sprayed on the surface of the metallic lithium. The amide can react with the metallic lithium to form a layer of artificial interface on the surface of the metallic lithium in advance, thereby protecting the metallic lithium negative electrode and improving the storage stability, service life and rate performance of the battery.

[0030] (2) The discharge rate of the battery made of lithium metal treated by the method of the present invention at 3C can reach more than 93.2%, the capacity retention rate after storage in a constant temperature environment of 45°C for 28 days can reach more than 89.2%, and the internal resistance change rate after storage in a constant temperature environment of 45°C for 28 days can reach less than 12.7%. By adjusting the mass concentration of amide in the amide solution, the discharge rate of the battery at 3C can reach 96.7%, the capacity retention rate after storage in a constant temperature environment of 45°C for 28 days can reach 94.2%, and the internal resistance change rate after storage in a constant temperature environment of 45°C for 28 days can reach 2.3%. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0032] Example 1

[0033] This embodiment provides a lithium metal processing method, the method comprising the following steps:

[0034] (1) mixing carbonamide and ethyl methyl carbonate to obtain an amide solution having a carbonamide mass concentration of 5%;

[0035] (2) Soaking the amide solution on the surface of the metal lithium sheet for 30 minutes to obtain treated metal lithium.

[0036] Example 2

[0037] This embodiment provides a lithium metal processing method, the method comprising the following steps:

[0038] (1) mixing N,N-dimethylformamide and ethyl methyl carbonate to obtain an amide solution having a mass concentration of 6% of N,N-dimethylformamide;

[0039] (2) Spraying the amide solution on the surface of the metal lithium strip for 20 minutes to obtain treated metal lithium.

[0040] Example 3

[0041] This embodiment provides a lithium metal processing method, the method comprising the following steps:

[0042] (1) mixing carbonamide and ethyl methyl carbonate to obtain an amide solution having a carbonamide mass concentration of 1%;

[0043] (2) Soaking the amide solution on the surface of the metal lithium sheet for 30 minutes to obtain treated metal lithium.

[0044] Example 4

[0045] This embodiment provides a lithium metal processing method, the method comprising the following steps:

[0046] (1) mixing carbonamide and ethyl methyl carbonate to obtain an amide solution having a carbonamide mass concentration of 12%;

[0047] (2) Soaking the amide solution on the surface of the metal lithium sheet for 30 minutes to obtain treated metal lithium.

[0048] Comparative Example 1

[0049] This comparative example provides a lithium metal processing method, which comprises the following steps:

[0050] (1) mixing ethylenediamine and ethyl methyl carbonate to obtain an ethylenediamine solution having an ethylenediamine mass concentration of 5%;

[0051] (2) Soaking the ethylenediamine solution on the surface of the metal lithium sheet for 30 minutes to obtain treated metal lithium.

[0052] Performance Testing:

[0053] The treated metal lithium material and manganese dioxide pole piece are assembled into button cells, and the newly prepared battery of the same group is discharged to 2.0V at 1C, and the discharge capacity is taken as the initial capacity of the battery. The capacity of 3C discharge to 2.0V and the percentage (%) of 1C discharge capacity are used as a method to measure the battery rate discharge performance. Before battery storage, the voltage, internal resistance and other parameters are tested. The newly prepared battery is placed in a constant temperature environment of 45℃ for 28 days, and then placed at room temperature for 2hrs to test the change in battery internal resistance. The battery capacity retention is tested by 1C discharge to 2.0V. The above data are used to calculate the capacity retention rate and internal resistance change rate.

[0054] Table 1

[0055]

[0056]

[0057] As can be seen from Table 1, from Examples 1-4, the discharge rate of the battery made of lithium metal treated by the method of the present invention at 3C can reach more than 93.2%, the capacity retention rate after storage in a constant temperature environment of 45°C for 28 days can reach more than 89.2%, and the internal resistance change rate after storage in a constant temperature environment of 45°C for 28 days can reach less than 12.7%. By adjusting the mass concentration of amide in the amide solution, the discharge rate of the battery at 3C can reach 96.7%, the capacity retention rate after storage in a constant temperature environment of 45°C for 28 days can reach 94.2%, and the internal resistance change rate after storage in a constant temperature environment of 45°C for 28 days can reach 2.3%.

[0058] By comparing Example 1 and Examples 3-4, it can be seen that the mass concentration of amide in the amide solution will affect the treatment effect of metallic lithium. When the mass concentration of amide in the amide solution is controlled at 2-10%, the treatment effect of metallic lithium is better. If the mass concentration of amide is too low, the capacity retention rate (calendar life) after high-temperature storage is low, and the internal resistance change rate is large. If the mass concentration of amide is too high, the capacity retention rate and internal resistance change rate after battery storage are not further improved.

[0059] By comparing Example 1 and Comparative Example 1, it can be seen that the present invention uses an amide solution to treat metallic lithium. Compared with amines, the unique carbonyl group (C=O) in the amide group is conjugated with the electrons on the nitrogen atom (N), which reduces the electron cloud density of the NH bond, so that the surface of the amide metal lithium negative electrode exhibits higher chemical activity, and can quickly form a dense and stable solid electrolyte interface layer on the surface of the metallic lithium, blocking the physical contact between the fresh metallic lithium and the solution components, thereby improving the stability of the metallic lithium.

[0060] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A lithium metal processing method, characterized in that: The method comprises the following steps: (1) mixing an amide and an organic solvent to obtain an amide solution; (2) coating the amide solution on the surface of metallic lithium to obtain treated metallic lithium; Based on the mass of the amide solution being 100%, the mass fraction of the amide in step (1) is 2 to 10%; The amide includes any one of carbonamide, N,N-dimethylformamide or halogenated amide or a combination of at least two thereof, and the organic solvent includes any one of carbonate, carboxylate, ether or nitriles or a combination of at least two thereof; The coating method in step (2) includes spraying and / or immersion, and the coating time is 5 to 60 minutes.

2. The method according to claim 1, characterized in that The organic solvent includes any one of dimethyl carbonate, ethyl methyl carbonate, propyl carbonate, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, ether, tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, acetonitrile, propionitrile, butyronitrile, adiponitrile or succinonitrile, or a combination of at least two thereof.

3. The method according to claim 1, characterized in that The coating humidity is ≤150 ppm.

4. The method according to claim 1, characterized in that The coating humidity is ≤50 ppm.

5. The method according to claim 1, characterized in that The metallic lithium in step (2) includes lithium sheets and / or lithium strips.

6. A metallic lithium negative electrode material, characterized in that: The metallic lithium negative electrode material is obtained by the lithium metal processing method according to any one of claims 1 to 5.

7. A negative electrode plate, characterized in that: The negative electrode plate comprises the metallic lithium negative electrode material as claimed in claim 6.

8. A lithium primary battery, characterized in that: The lithium primary battery comprises the negative electrode sheet as claimed in claim 7.

Citation Information

Patent Citations

  • Lithium metal primary cell negative flake

    CN102623670A

  • Lithium / lithium alloy composite negative electrode for high-power primary battery, preparation method and battery

    CN111952571A

  • Lithium metal negative electrode, preparation method thereof and lithium metal battery

    CN111490250A

  • Metal lithium negative electrode with polyimide protective coating as well as preparation and application thereof

    CN111653726A

  • Lithium Metal Battery Comprising Polyimide Film And Method of Producing Thereof

    KR1020090055224A