A water-lubricated water-guided bearing device and an environmentally friendly water-lubricated rust remover used therein
Through modified polytetrafluoroethylene resin and coating technology, as well as the use of environmentally friendly anti-rust particles, the problem of water guide bearing leakage and pollution is solved, higher sealing and anti-rust effects are achieved, and strict environmental protection requirements are met.
Patent Information
- Application Number
- CN202111676282.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The water guide bearing in the vertical hydroelectric generator unit can easily cause lubricant leakage during operation, causing water source pollution. Moreover, the existing sodium nitrate aqueous solution is slightly toxic and difficult to meet strict environmental protection requirements.
The water guide bearing is made of modified polytetrafluoroethylene resin, and its surface is plated with heat-insulating vanadium and chromium nitride aluminum plating. It is combined with a water-lubricating rust remover prepared from environmentally friendly anti-rust particles to improve sealing and anti-rust effects. Reduce the risk of water contamination.
It effectively avoids corrosion of water guide bearings in water, reduces the need for water-based rust inhibitors, achieves longer-lasting anti-rust and antibacterial effects, avoids water pollution, and meets strict environmental standards.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of vertical hydro-turbine generator sets, and in particular to a water-lubricated water-guided bearing device and an environmentally friendly water-lubricated rust remover used therein. Background Art
[0002] As the world's environmental protection requirements become increasingly strengthened and improved, today's hydropower stations must not only meet the ecological flow requirements of the river basin where the power station is located during normal operation, but also need to avoid protecting the water source in the flow path from secondary pollution during the power generation process. The clean energy powered by water - hydropower stations will face huge challenges and tests.
[0003] Hydroelectric power stations usually use turbine generator sets. At present, turbine generator sets will inevitably cause certain pollution to water sources. The main reasons why turbine generator sets cause water pollution are: lubricating oil in power generation equipment and operating oil in the runner of propeller units.
[0004] A vertical hydro-turbine generator set in the related art includes a generator rotor, a turbine main shaft, a runner and bearing equipment, wherein the bearing equipment includes a thrust bearing, an upper guide bearing, a lower guide bearing and a water guide bearing. The lubrication method is full oil immersion or a spiral oil tank pump oil or a rotary hole pump oil or a pitot tube pump oil. The upper and lower bearings and the water guide bearings of the vertical unit are subjected to relatively simple forces, with a low unit pressure and are easier to handle. Although the thrust, upper guide, lower guide and water guide bearings of each gear in the vertical unit are also above the ground, once leaked oil mist and oil droplets appear, because the thrust, upper guide and lower guide have a certain height space from the turbine layer, they can be handled in the same way as the horizontal unit. However, once oil mist or oil droplets appear in the water guide bearing, because the water guide bearing is located at the upper end of the main shaft seal, it is difficult to handle after leakage. The main reasons are: first, because it is in the machine pit, it is not easy to find; second, it is low in position and difficult to handle, and it will enter the downstream along with the drainage of the main shaft seal, causing secondary pollution to the water source.
[0005] In order to solve the above problems, the applicant has improved the water-lubricated water-guide bearing device of the vertical unit, such as a water-lubricated water-guide bearing disclosed in announcement number CN212177316U, which includes a rotating oil pan and a pitot tube, the outer wall of the rotating oil pan is inlaid with bolts, and the lower side of the bolts is provided with a rubber strip, the inner end of the rotating oil pan is provided with a vertical shaft, and the upper end of the vertical shaft is connected to an edge plate, a bearing seat is provided in the middle position of the edge plate, and a vertical steel pipe is placed on the top of the vertical shaft, a temperature measuring resistor is installed on the right side of the vertical steel pipe, and a bearing cover is provided above the cooler temperature measuring resistor, an inspection cover is filed on the left side of the bearing cover, a screw is provided in the middle position of the bearing cover, and an inspection orifice plate is provided on the outer surface of the bearing cover. The oil pan and the rubber strip can be rotated to squeeze them through the threaded fastening to fill the gap to ensure that the connection part has good airtightness, and the sealing of the connection structure can be maintained to prevent the leakage of the internal lubricating liquid and avoid polluting the downstream river. At present, the internal lubricating liquid of the organization adopts a low-concentration sodium nitrate aqueous solution.
[0006] Regarding the above-mentioned water-lubricated water-guided bearing structure, the applicant found that the following problems still exist: the sodium nitrate aqueous solution used is slightly toxic. Although the overall sealing is improved, a small amount of sodium nitrate aqueous solution will inevitably leak out. However, under the current environmental protection requirements of many regions, if pollutants appear on the downstream water surface, the hydropower station will face heavy penalties at the least, and the hydropower station will face closure at the worst. If it is used as a water source for urban and residential water use, the requirements are higher. The water-lubricated water-guided bearing structure needs further improvement. Summary of the invention
[0007] In order to solve the problems existing in the related art, the present application provides a water-lubricated water-guided bearing device and an environmentally friendly water-lubricated rust remover used therein.
[0008] In the first aspect, a water-lubricated water-guided bearing device provided in the present application is realized through the following technical scheme: a water-lubricated water-guided bearing device, comprising a water-lubricated water-guided bearing shell, the water-lubricated water-guided bearing shell is made of modified polytetrafluoroethylene resin; the surface of the water-lubricated water-guided bearing shell is sequentially formed with a heat-retaining vanadium coating layer and a chromium nitride aluminum coating layer through a physical vapor deposition PVD process.
[0009] By adopting the above-mentioned technical scheme, the present application improves the water-lubricated water-guided bearing, prepares the water-guided bearing with modified polytetrafluoroethylene, and then plates a heat-retaining vanadium coating and a chromium aluminum nitride coating on the inner surface of the water-guided bearing, thereby effectively improving the heat resistance stability and mechanical strength of the water-guided bearing made of modified polytetrafluoroethylene material, so that it meets the requirements as a water-guided bearing. Therefore, the water-lubricated water-guided bearing prepared in the present application can avoid the corrosion of the water-guided bearing by dissolved oxygen in the water, and at the same time reduce the requirements for water-based rust inhibitors.
[0010] Preferably, the modified polytetrafluoroethylene resin is prepared from the following raw materials in parts by weight: 100 parts of polytetrafluoroethylene resin, 1-5 parts of nano-fumed silica, 1-3 parts of dispersant, and 3-10 parts of alumina-carbon nanotube hybrid filler.
[0011] By adopting the above technical scheme, the dispersant is used to evenly disperse the nano-gas-phase silica and the alumina-carbon nanotube hybrid filler in the system and make the nano-gas-phase silica, the alumina-carbon nanotube hybrid filler and the polytetrafluoroethylene resin have good compatibility. Nano-gas-phase silica is used to improve the wear resistance and mechanical strength of the modified polytetrafluoroethylene resin. The alumina-carbon nanotube hybrid filler is used to improve the heat stability and mechanical strength of the modified polytetrafluoroethylene resin while ensuring the insulation performance of the modified polytetrafluoroethylene resin, thereby preparing a water-lubricated water-guide bearing that meets the requirements of a vertical hydro-turbine generator set. The water-lubricated water-guide bearing prepared from the modified polytetrafluoroethylene resin has good wear resistance and insulation, and has a certain thermal conductivity, which reduces the overall thermal expansion coefficient and improves the overall heat resistance stability.
[0012] Preferably, the preparation method of the modified polytetrafluoroethylene resin comprises the following steps: step 1, accurately measuring the polytetrafluoroethylene resin according to the ratio, drying and setting aside; step 2, accurately measuring the nano-fumed silica, dispersant and alumina-carbon nanotube hybrid filler according to the ratio, mixing them evenly to obtain a modified powder; step 3, evenly mixing the modified powder in step 2 and the polytetrafluoroethylene resin in step 1, melt-extruding, cooling, granulating and drying to obtain the modified polytetrafluoroethylene resin.
[0013] By adopting the above technical scheme, modified polytetrafluoroethylene resin granules for preparing water-lubricated water-guided bearings can be obtained, thereby ensuring the quality of the prepared water-lubricated water-guided bearings to meet the requirements of vertical hydro-turbine generator sets.
[0014] Preferably, the processing technology of the heat-retaining vanadium coating comprises the following steps: step one, polishing, ultrasonic cleaning, and drying the surface of the water-lubricated water-guided bearing in sequence; step two, using a PVD arc coating system to perform cathode arc plasma deposition on the surface of the water-lubricated water-guided bearing in step two to form a heat-retaining vanadium coating.
[0015] By adopting the above technical solution, the heat-retaining vanadium coating can prevent the inner surface of the water-lubricated water-guided bearing from overheating, playing the role of heat insulation and protection of the water-lubricated water-guided bearing. In addition, it can reduce the damage to the water-lubricated water-guided bearing caused by the internal stress caused by overcooling and overheating, and improve the overall service life of the water-lubricated water-guided bearing.
[0016] Preferably, the processing technology of the chromium nitride aluminum coating comprises the following steps: step one, polishing, ultrasonic cleaning, and drying the heat-retaining vanadium coating on the surface of the water-lubricated water-guided bearing in sequence; step two, using a PVD arc coating system to perform cathode arc plasma deposition on the surface of the heat-retaining vanadium coating of the water-lubricated water-guided bearing in step two to form a chromium nitride aluminum coating; step three, grinding and polishing the surface to obtain a finished product.
[0017] By adopting the above technical solution, the chromium nitride aluminum coating plays an anti-oxidation and anti-friction role. At the same time, the chromium nitride aluminum coating avoids a low friction coefficient, which can reduce the heat generated by the friction between the water body and the chromium nitride aluminum coating, protect the water-lubricated water-guided bearing, and improve the overall service life of the water-lubricated water-guided bearing.
[0018] In the second aspect, the present application provides an environmentally friendly water-lubricated rust remover for use in a water-lubricated water-guided bearing device, which is achieved through the following technical solutions:
[0019] An environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water, 0.5-2 parts of environmentally friendly rust-proof particles; the particle size of the environmentally friendly rust-proof particles is 50-300 microns; the environmentally friendly rust-proof particles are prepared from the following raw materials in parts by weight: 2-10 parts of ascorbic acid, 1-5 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.1-0.5 parts of chitosan antibacterial agent, 30-50 parts of porous adsorption particles, 2-8 parts of glyceryl monostearate emulsifier, 5-10 parts of coating agent, and 30-35 parts of ethanol.
[0020] By adopting the above technical scheme, on the basis of the water-lubricated and water-guided bearing made of polytetrafluoroethylene resin material in this application, combined with the environmentally friendly anti-rust particles developed in this application, adding 0.5-2 parts into the water body can achieve good anti-rust and antibacterial effects, and the components in the environmentally friendly anti-rust particles are pollution-free to the environment and have good environmental performance.
[0021] Preferably, the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 2-10 parts of ascorbic acid, 1-3 parts of sodium carbonate, 1-5 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.1-0.5 parts of chitosan antibacterial agent, 30-50 parts of porous adsorption particles, 2-8 parts of monostearate glycerol emulsifier, 5-10 parts of coating agent, and 30-35 parts of ethanol.
[0022] By adopting the above technical scheme, sodium carbonate is added to the environmentally friendly anti-rust particles because ascorbic acid slowly released in water will produce acidity, and sodium carbonate is used to neutralize the acid, thereby avoiding acid corrosion of the rotating shaft, so that the environmentally friendly water-lubricated rust remover prepared in this application has a better and more lasting anti-rust effect.
[0023] Preferably, the method for preparing the environmentally friendly rust-proof particles comprises the following steps:
[0024] Step 1, preparing porous adsorption particles;
[0025] Step 2: Under stirring, porous adsorption particles accounting for 50-60% of the total mass of the porous adsorption particles and glyceryl monostearate emulsifier are added to ethanol in sequence, heated to 70-75° C. and stirred for 5-10 minutes, then cooled to 40-45° C., 4,5-dichloro-N-octyl-4-isothiazoline-3-one, chitosan antibacterial agent and ascorbic acid accounting for 60-80% of the mass are added, and an emulsion is obtained under high-speed shear stirring at 2800-3200 rpm;
[0026] Step 3, spraying the emulsion on the remaining porous adsorption particles, spraying low-temperature granulation, to obtain particles;
[0027] Step 4: The obtained particles are vacuum dried at 40-50°C for 3-4 hours, and the moisture content of the particles after drying is 10-15%. The particles are cooled to room temperature and then sieved;
[0028] Step 5: In a boiling fluidized bed, a coating machine coats the particles with the remaining ascorbic acid and the coating agent mixture to obtain a finished product.
[0029] By adopting the above technical scheme, after the coating agent in the prepared environmentally friendly anti-rust particles is dissolved in water, ascorbic acid and 4,5-dichloro-N-octyl-4-isothiazoline-3-one are slowly released in the water body, ascorbic acid can remove dissolved oxygen in the water body, thereby playing a good anti-rust effect, 4,5-dichloro-N-octyl-4-isothiazoline-3-one has a good antibacterial effect, and can purify water quality by itself, and can be degraded in natural water bodies, so that the present application has more lasting anti-rust and antibacterial properties.
[0030] Preferably, the method comprises the following steps:
[0031] Step 1, preparing porous adsorption particles;
[0032] Step 2: Under stirring, porous adsorption particles accounting for 50-60% of the total mass of the porous adsorption particles and glyceryl monostearate emulsifier are added to ethanol in sequence, heated to 70-75° C. and stirred for 5-10 minutes, then cooled to 40-45° C., 4,5-dichloro-N-octyl-4-isothiazoline-3-one, chitosan antibacterial agent and ascorbic acid accounting for 60-80% of the mass are added, and an emulsion is obtained under high-speed shear stirring at 2800-3200 rpm;
[0033] Step 3, spraying the emulsion on the remaining porous adsorption particles, spraying low-temperature granulation, to obtain particles;
[0034] Step 4: The obtained particles are vacuum dried at 40-50°C for 3-4 hours, and the moisture content of the particles after drying is 10-15%. The particles are cooled to room temperature and then sieved;
[0035] Step 5, in a boiling fluidized bed, the coating machine first coats the particles with a mixture of the remaining coating agent and the remaining ascorbic acid, and then coats the particles with a mixture of the coating agent and sodium carbonate accounting for 40-50% of the total mass of the coating agent for a second time to obtain the finished product.
[0036] By adopting the above technical scheme, after the coating agent in the prepared environmentally friendly anti-rust particles is dissolved in water, ascorbic acid and 4,5-dichloro-N-octyl-4-isothiazoline-3-one are first slowly released into the water body, and then sodium carbonate and 4,5-dichloro-N-octyl-4-isothiazoline-3-one are slowly released into the water body. Ascorbic acid can remove dissolved oxygen in the water body, thereby playing a good anti-rust effect, but the water body is weakly acidic, and the slowly released sodium carbonate has a great effect on the H + Neutralization is carried out to avoid acid corrosion of the rotating shaft, so that the environmentally friendly water-lubricated rust remover prepared in the present application has a better and more lasting anti-rust effect.
[0037] In summary, this application has the following advantages:
[0038] 1. The water-lubricated water-guided bearing in the present application meets the requirements for being a water-guided bearing for a vertical unit, can avoid corrosion of the water-guided bearing by dissolved oxygen in the water, and at the same time reduces the requirements for water-based rust inhibitors.
[0039] 2. The environmentally friendly water-lubricated rust remover in this application not only has a long-lasting anti-rust and bactericidal effect, but also its components will not cause secondary pollution to the water body, can purify the water quality, and has more environmental advantages. DETAILED DESCRIPTION
[0040] The present application is further described in detail below in conjunction with embodiments.
[0041] Preparation Example
[0042] Preparation Example 1
[0043] The preparation method of aluminum oxide-carbon nanotube hybrid filler comprises the following steps:
[0044] Step 1: Add 2.907 g of nickel nitrate hexahydrate and 2.794 g of aluminum powder into 1 L of deionized water, then drop 500 ml of a 0.04 mol / L sodium hydroxide solution into the solution under stirring with a magnetic stirrer at 200 rpm to react and generate a Ni(OH)2 / Al binary colloid with a mass percentage of Ni to Al of 1:4.76;
[0045] Step 2: Dehydrate the obtained binary colloid in an air atmosphere furnace at 400°C for 4 hours, with the furnace heating rate being 8°C / min, thereby obtaining a NiO / Al2O3 catalyst precursor;
[0046] Step three, take NiO / Al2O3 catalyst precursor and spread it in a quartz boat, and place the quartz boat in the constant temperature zone in the middle of the quartz reaction tube, first introduce nitrogen into the reaction tube to exclude air, raise the temperature to 400°C at a heating rate of 8°C / min, then introduce hydrogen at 200ml / min for 2 hours to reduce NiO / Al2O3 to Ni / Al2O3, stop introducing hydrogen, raise the furnace temperature to 800°C, then introduce a mixed gas of methane and nitrogen (VCH4 / VN2=60 / 540ml / min), react at 800°C for 0.5 hour, stop introducing the mixed gas, and then reduce the furnace temperature to room temperature 20°C in a mixed atmosphere of nitrogen and hydrogen (VN2 / VH2=75 / 60ml / min) to obtain a CNTs-Al2O3 hybrid filler with a carbon nanotube mass content of 60%, a nickel content of 4%, and an alumina aluminum content of 36%.
[0047] Preparation Example 2
[0048] The modified polytetrafluoroethylene resin is prepared from the following raw materials in parts by weight: 100 parts of polytetrafluoroethylene resin (DuPont PTFE, injection molding grade, purchased from Guangzhou Jingchen Plastic Chemical Co., Ltd.), 3 parts of nano-fumed silica (CAS No.: 10279-57-9, Jinan Chaoyixing Chemical Co., Ltd.), 2 parts of dispersant - Degussa non-ionic wetting and dispersing agent BREAK-THRUDA646, and 6 parts of alumina-carbon nanotube hybrid filler in Preparation Example 1.
[0049] The preparation method of modified polytetrafluoroethylene resin comprises the following steps:
[0050] Step 1: accurately measure 10 kg of polytetrafluoroethylene resin according to the ratio, dry it at 80° C. for 4 hours, and set it aside;
[0051] Step 2: accurately weigh 0.3 kg of nano fumed silica, 0.2 kg of Degussa nonionic wetting and dispersing agent BREAK-THRUDA646, and 0.6 kg of the alumina-carbon nanotube hybrid filler in Preparation Example 1 according to the ratio, and mix and disperse them at 300 rpm for 10 minutes to obtain a modified powder;
[0052] Step 3, the modified powder in step 2 and the polytetrafluoroethylene resin in step 1 are mixed and dispersed at 300 rpm for 2 minutes, added into a twin-screw extruder for melt extrusion, the temperatures of the five heating sections of the twin-screw extruder are 340°C, 360°C, 380°C, 382°C, and 382°C, respectively, the extruded material is introduced into cold water for cooling, introduced into a granulator for granulation, and the obtained granules are placed at 100°C for drying to obtain modified polytetrafluoroethylene resin.
[0053] Preparation Example 3
[0054] The coating agent is prepared from the following raw materials: 7% acrylic resin No. Ⅱ (content 99%, Wuhan Kemik Biopharmaceutical Technology Co., Ltd.), 2.5% diethyl phthalate (content ≥ 99% from Sinopec), 3% polysorbate-80 (CAS: 9005-65-6, model: T-80, content ≥ 99%), 6% caprylic acid triglyceride, 1.5% montmorillonite (pharmaceutical grade CAS No.: 1318-93-0), 80% anhydrous ethanol coating agent, comprising the following steps: adding 1.6 kg of anhydrous ethanol into a liquid preparation tank, starting stirring at a stirring speed of 150 rpm, sequentially adding 0.14 kg of acrylic resin No. II, 0.05 kg of diethyl phthalate, 0.06 kg of polysorbate-80, 0.12 kg of caprylic acid triglyceride, and 0.03 kg of montmorillonite, heating to 45° C., stirring for 5 minutes, and obtaining the coating agent.
[0055] Preparation Example 4
[0056] The environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 2 parts of ascorbic acid, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of glyceryl monostearate, 6 parts of the coating agent in Preparation Example 3, and 30 parts of anhydrous ethanol.
[0057] The preparation of porous adsorption particles comprises the following steps:
[0058] Step 1, weigh 7 kg of 4A molecular sieve powder according to the ratio, activate it at 400°C for 2 hours, cool it naturally to room temperature, and set it aside;
[0059] Step 2: weigh 7 g of deionized water, 1.5 kg of 4A molecular sieve, and 1.2 kg of glyceryl monostearate according to the ratio, and emulsify and disperse them at 2800 rpm for 30 min to obtain an emulsion;
[0060] Step 3: The emulsion in step 2 is sprayed on 5.5 kg of 4A molecular sieve using a pressure pump, and sprayed at 60°C for low-temperature granulation;
[0061] Step 4: The obtained particles are dried at 50° C. under vacuum (200 mbar) for 4 h, and the moisture content of the particles after drying is controlled between 13% and 15%;
[0062] Step 5: calcine the particles dried in step 4 at 500° C. in a 5% hydrogen-argon atmosphere with a gas pressure of 0.3 MPa for 5.0 h, cool to room temperature, and then sieve with 100 mesh.
[0063] The method for preparing environmentally friendly anti-rust particles comprises the following steps:
[0064] Step 1, under stirring, add 400g of porous adsorption particles and 120g of monostearate glycerol emulsifier to 600g of ethanol in sequence, heat to 70°C and stir for 5min, then cool to 40°C, add 40g of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 4g of chitosan antibacterial agent and 80% of the total mass of ascorbic acid (weighing mass 32g), and obtain an emulsion under high-speed shear stirring at 3000rpm;
[0065] Step 2: spray the emulsion onto 300 g of porous adsorption particles, spray low-temperature granulation at 60° C., and cool the obtained particles;
[0066] Step 3, the obtained particles are vacuum dried at 45°C for 4 hours, the moisture content of the particles is controlled at 10-15% after drying, and the particles are sieved with 80 mesh after cooling to room temperature;
[0067] Step 4: In a boiling fluidized bed, a coating machine uses the remaining 8 g of ascorbic acid and 120 g of the coating agent mixture in Preparation Example 3 to coat the sieved particles in Step 3 to obtain a finished product.
[0068] Preparation Example 5
[0069] The difference between Preparation Example 5 and Preparation Example 4 is that the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 5 parts of ascorbic acid, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of monostearate glyceryl, 6 parts of the coating agent in Preparation Example 3, and 30 parts of anhydrous ethanol.
[0070] Preparation Example 6
[0071] The difference between Preparation Example 6 and Preparation Example 4 is that the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 10 parts of ascorbic acid, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of monostearate glyceryl, 6 parts of the coating agent in Preparation Example 3, and 30 parts of anhydrous ethanol.
[0072] Preparation Example 7
[0073] The difference between Preparation Example 7 and Preparation Example 4 is that the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 6 parts of ascorbic acid, 2 parts of sodium carbonate, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of monostearate glyceryl, 8 parts of the coating agent in Preparation Example 3, and 35 parts of anhydrous ethanol.
[0074] The method for preparing environmentally friendly anti-rust particles comprises the following steps:
[0075] Step 1, under stirring, add 400g of porous adsorption particles and 120g of monostearate glycerol emulsifier to 700g of ethanol in sequence, heat to 70°C and stir for 5min, then cool to 40°C, add 40g of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 4g of chitosan antibacterial agent and 80% of the total mass of ascorbic acid (weighing mass 96g), and obtain an emulsion under high-speed shear stirring at 3000rpm;
[0076] Step 2: spray the emulsion onto 300 g of porous adsorption particles, spray low-temperature granulation at 60° C., and cool the obtained particles;
[0077] Step 3, the obtained particles are vacuum dried at 45°C for 4 hours, the moisture content of the particles is controlled at 10-15% after drying, and the particles are sieved with 80 mesh after cooling to room temperature;
[0078] Step 4, in a boiling fluidized bed, the coating machine uses 40g of sodium carbonate and 80g of the coating agent mixture in Preparation Example 3 to perform a first coating treatment on the sieved particles in Step 3, and then uses 80g of the coating agent and the remaining 24g of ascorbic acid to perform a second coating treatment on the particles to obtain finished environmentally friendly rust-proof particles.
[0079] Preparation Example 8
[0080] The difference between Preparation Example 8 and Preparation Example 4 is that the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 1 part of ascorbic acid, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of monostearate glyceryl, 6 parts of the coating agent in Preparation Example 3, and 30 parts of anhydrous ethanol.
[0081] Preparation Example 9
[0082] The difference between Preparation Example 9 and Preparation Example 4 is that the environmentally friendly anti-rust particles are prepared from the following raw materials in parts by weight: 15 parts of ascorbic acid, 2 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.2 parts of chitosan antibacterial agent, 35 parts of porous adsorption particles, 6 parts of monostearate glyceryl, 6 parts of the coating agent in Preparation Example 3, and 30 parts of anhydrous ethanol.
[0083] Example
[0084] Example 1
[0085] The present application discloses a water-lubricated water-guided bearing device, which includes a water-lubricated water-guided bearing bush. The water-lubricated water-guided bearing bush is prepared from the modified polytetrafluoroethylene resin in Preparation Example 2.
[0086] The surface of the water-lubricated water-guided bearing is sequentially formed with a heat-retaining vanadium coating layer and a chromium-aluminum nitride coating layer by a physical vapor deposition (PVD) process. The processing technology of the heat-retaining vanadium coating layer and the chromium-aluminum nitride coating layer includes the following steps:
[0087] Step 1, polishing, ultrasonic cleaning and drying the surface of the water-lubricated water-guided bearing in sequence;
[0088] Step 1.1, the inner surface of the water-lubricated water-guided bearing is polished with 200#, 500#, 800# and 1500# sandpaper in sequence, and then the powder on the surface of the water-lubricated water-guided bearing is blown off with an air gun;
[0089] Step 1.2, the water-lubricated water-guided bearing is ultrasonically cleaned, the ultrasonic frequency is 44kHz, the power is 400w, and the cleaning time is 30min;
[0090] Step 1.3, drying at 80°C for 30 min, set aside;
[0091] Step 2, using a PVD arc coating system to perform cathode arc plasma deposition on the water-lubricated water-guided bearing that has been dried in step 1.3;
[0092] Step 2.1, install the water-lubricated water-guided bearing on the rotating sample table in the vacuum chamber, install the vanadium target on the cathode arc evaporator, and evacuate the vacuum chamber to a vacuum degree of 1.0*10 -3 Pa, introduce argon gas into the vacuum chamber, and adjust the argon gas flow rate to make the vacuum degree of the vacuum chamber 4.0*10 -1 Pa;
[0093] Step 2.2, turn on the filament, filament magnetic field, and acceleration power supply, adjust the substrate bias to -600 V, perform surface bombardment glow cleaning for 30 minutes, and no sparks are observed on the substrate;
[0094] Step 2.3, control the flux of argon and nitrogen, nitrogen flow rate 60sccm, argon 40sccm, nitrogen partial pressure 60%, adjust the vacuum degree of the vacuum chamber to 2*10 -1 Pa, the substrate bias is adjusted to -200V, the duty cycle of the substrate bias is 45:55, and then the target magnetic field is turned on to ignite the vanadium target. The arc working voltage is 22V, the arc current is adjusted to 120A, the deposition time is 1h, and it is naturally cooled to room temperature. A heat-retaining vanadium coating is formed on the surface of the water-lubricated water-guided bearing.
[0095] Step 3, polishing, ultrasonic cleaning, and drying the surface of the heat-retaining vanadium coating of the water-lubricated water-guided bearing in sequence;
[0096] Step 3.1, polishing: first use an air gun with compressed air as the air source to blow air on the surface of the water-lubricated water-guided bearing to remove the dust on the surface, and then use 800#, 1000#, 1200#, 1500#, and 2000# sandpaper to polish in sequence. Before changing different types of sandpaper, use an air gun to blow away the polishing powder; after sandpaper polishing, use 800-mesh screened chromium trioxide grinding powder and flannel cloth for fine polishing; first observe with the naked eye, if no visible oil, grease, residual oxide scale, rust, and residual paint and other dirt are observed on the surface, then test the cleanliness of the surface of the water-lubricated water-guided bearing according to the Sa test standard, when the detected cleanliness reaches Sa1 level, complete the polishing treatment, wipe with cotton cloth dipped in medical alcohol, and wipe the surface of the aluminum profile hot extrusion die repeatedly until there is no foreign matter on the cotton cloth surface of the aluminum profile hot extrusion die surface;
[0097] Step 3.2, placing the water-lubricated water-guided bearing in an ultrasonic cleaning machine, performing ultrasonic cleaning at 45kHz for 30 minutes, placing it in an oven, and drying it at 80°C for 1.0 hour under a nitrogen atmosphere;
[0098] Step 4, using a PVD arc coating system to perform cathode arc plasma deposition on the water-lubricated water-guided bearing that has been dried in step 3.2;
[0099] Step 4.1, install the water-lubricated water-guided bearing on the rotating sample table in the vacuum chamber, install the vanadium target on the cathode arc evaporator, and evacuate the vacuum chamber to a vacuum degree of 1.0*10 -3 Pa, introduce argon gas into the vacuum chamber, and adjust the argon gas flow rate to make the vacuum degree of the vacuum chamber 4.0*10 -1 Pa;
[0100] Step 4.2, turn on the filament, filament magnetic field, and acceleration power supply, adjust the substrate bias to -700 V, perform surface bombardment glow cleaning for 30 minutes, and no sparks are observed on the substrate;
[0101] Step 4.3, control the flux of argon and nitrogen, nitrogen flow rate 65sccm, argon 35sccm, nitrogen partial pressure 65%, adjust the vacuum degree of the vacuum chamber to 5*10 -1 Pa, the substrate bias is adjusted to -200V, the duty cycle of the substrate bias is 43:57, and then the target magnetic field is turned on to ignite the chromium-aluminum target. The arc working voltage is 22V, the arc current is adjusted to 100A, the deposition time is 2h, and it is naturally cooled to room temperature; Step five, a sandblasting machine is used to perform surface sandblasting on the water-lubricated water-guided bearing. The sandblasting is performed using corundum screened with a particle size of 800 mesh. The cleanliness of the surface of the aluminum profile hot extrusion die is detected according to the Sa detection standard until the detected cleanliness reaches Sa2.5 level.
[0102] An environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water and 0.5 parts of the environmentally friendly rust-proof particles in Preparation Example 4. The particle size of the environmentally friendly rust-proof particles is 180 microns.
[0103] A method for preparing an environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device: weigh 10 kg of deionized water, add 50 g of the environmentally friendly anti-rust particles in Preparation Example 4 into the deionized water at a speed of 5 g / min, and control the stirring speed at 1600 rpm. After the addition is completed, maintain the stirring speed and stir for another 5 minutes to obtain a finished environmentally friendly water-lubricated rust remover.
[0104] Example 2
[0105] The difference between Example 2 and Example 1 is that an environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water and 1.25 parts of the environmentally friendly rust-proof particles in Preparation Example 4. The particle size of the environmentally friendly rust-proof particles is 180 microns.
[0106] Example 3
[0107] The difference between Example 3 and Example 1 is that an environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water and 2 parts of the environmentally friendly rust-proof particles in Preparation Example 4. The particle size of the environmentally friendly rust-proof particles is 180 microns.
[0108] Example 4
[0109] The difference between Example 4 and Example 1 is that the environmentally friendly anti-rust particles are replaced by the environmentally friendly anti-rust particles in Preparation Example 5.
[0110] Example 5
[0111] The difference between Example 5 and Example 1 is that the environmentally friendly anti-rust particles are replaced by the environmentally friendly anti-rust particles in Preparation Example 6.
[0112] Example 6
[0113] The difference between Example 6 and Example 1 is that the environmentally friendly anti-rust particles are replaced by the environmentally friendly anti-rust particles in Preparation Example 7.
[0114] Comparative Example
[0115] Comparative Example 1
[0116] The difference between Comparative Example 1 and Example 1 is that the environmentally friendly anti-rust particles are replaced by the environmentally friendly anti-rust particles in Preparation Example 8.
[0117] Comparative Example 2
[0118] The difference between Comparative Example 2 and Example 1 is that the environmentally friendly anti-rust particles are replaced by the environmentally friendly anti-rust particles in Preparation Example 9.
[0119] Comparative Example 3
[0120] The difference between Comparative Example 3 and Example 1 is that an environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water and 0.2 parts of the environmentally friendly rust-proof particles in Preparation Example 4. The particle size of the environmentally friendly rust-proof particles is 180 microns.
[0121] Comparative Example 4
[0122] The difference between Comparative Example 4 and Example 1 is that an environmentally friendly water-lubricated rust remover used in a water-lubricated water-guided bearing device is prepared from the following raw materials in parts by weight: 100 parts of deionized water and 3 parts of the environmentally friendly rust-proof particles in Preparation Example 4. The particle size of the environmentally friendly rust-proof particles is 180 microns.
[0123] Performance testing
[0124] Detection method / test method
[0125] 1. Test the dissolved oxygen content in the environmentally friendly water-lubricated rust remover using a dissolved oxygen meter at a room temperature of 25.0°C ± 0.2°C.
[0126] 2. Test the pH value change of environmentally friendly water-lubricated rust remover using an online pH meter. The test room temperature is 25.0℃±0.2℃.
[0127] Data analysis
[0128] project Dissolved oxygen content determination mg / L Prepare water 8.82 Example 1 0.32 Example 2 0.24 Example 3 0.19 Example 4 0.20 Example 5 0.18 Example 6 0.22 Comparative Example 1 1.3 Comparative Example 2 0.20 Comparative Example 3 0.84 Comparative Example 4 0.16
[0129] 0min 30min 1.0h 3.0h 6.0h 12h 24h Example 1 7.1 7.0 6.9 6.9 6.8 6.8 6.7 Example 2 7.2 7.1 7.0 6.8 6.7 6.7 6.6 Example 3 7.0 6.9 6.8 6.7 6.6 6.6 6.5 Example 4 7.1 7.0 6.8 6.7 6.7 6.7 6.6 Example 5 7.1 6.9 6.8 6.7 6.6 6.6 6.5 Example 6 7.2 7.4 7.7 7.5 7.3 7.2 7.1 Comparative Example 1 7.0 6.9 6.9 6.9 6.8 6.8 6.7 Comparative Example 2 7.2 7.0 6.8 6.7 6.6 6.5 6.4 Comparative Example 3 7.1 7.0 7.0 6.9 6.8 6.8 6.8 Comparative Example 4 7.2 7.1 7.0 6.8 6.7 6.6 6.5
[0130] It can be seen from Examples 1-6 and Comparative Examples 1-4 and Table 1 that the dissolved oxygen in the environmentally friendly water-lubricated rust remover of Examples 1-6 is controlled at 0.18-0.32 mg / L, and the dissolved oxygen removal rate is controlled at 96.4-97.8%. Therefore, the environmentally friendly water-lubricated rust remover in this application has a good rust removal effect and good environmental performance, and will not cause secondary pollution to the water body.
[0131] Combining Examples 1-6 and Comparative Examples 1-4 and Table 2, it can be seen that the pH value of the environmentally friendly water-lubricated rust remover prepared in Example 6 is controlled at neutral or weak alkaline, which effectively reduces the probability of acidic corrosion and achieves a better rust removal effect.
[0132] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An environmentally friendly water-lubricated rust remover used in water-lubricated water-guided bearing devices, Features: The environmentally friendly rust-proof particles are prepared from the following raw materials in parts by weight: 100 parts of deionized water, 0.5-2 parts of environmentally friendly rust-proof particles; the particle size of the environmentally friendly rust-proof particles is 50-300 microns; the environmentally friendly rust-proof particles are prepared from the following raw materials in parts by weight: 2-10 parts of ascorbic acid, 1-3 parts of sodium carbonate, 1-5 parts of 4,5-dichloro-N-octyl-4-isothiazoline-3-one, 0.1-0.5 parts of chitosan antibacterial agent, 30-50 parts of porous adsorption particles, 2-8 parts of monostearate glycerol emulsifier, 5-10 parts of coating agent, and 30-35 parts of ethanol; The method for preparing the environmentally friendly rust-proof particles comprises the following steps: Step 1, preparing porous adsorption particles; Step 2: Under stirring, add porous adsorption particles accounting for 50-60% of the total mass of the porous adsorption particles and glyceryl monostearate emulsifier to ethanol in sequence, heat to 70-75° C. and stir for 5-10 minutes, then cool to 40-45° C., add 4,5-dichloro-N-octyl-4-isothiazoline-3-one, chitosan antibacterial agent and ascorbic acid accounting for 60-80% of the mass, and obtain an emulsion under high-speed shear stirring at 2800-3200 rpm; Step 3, spraying the emulsion on the remaining porous adsorption particles, spraying low-temperature granulation, to obtain particles; Step 4: The obtained particles are vacuum dried at 40-50°C for 3-4 hours, and the moisture content of the particles after drying is 10-15%. After cooling to room temperature, the particles are sieved; Step 5, in a boiling fluidized bed, the coating machine first coats the particles with a mixture of the remaining coating agent and the remaining ascorbic acid, and then coats the particles for a second time with a mixture of the coating agent and sodium carbonate accounting for 40-50% of the total mass of the coating agent, to obtain the finished product.
Citation Information
Patent Citations
Water-lubricated water guide bearing
CN212177316U
Marine anti-fouling coating
CN104946052A
Water-lubricated bearing material
CN107110212A
Environment-friendly water-based double-component polyurethane anti-corrosion finishing paint and preparation method thereof
CN108912995A
Water lubricated bearing or water lubricated seal
CN1166576A