A kind of easy-opening controllable biodegradable blown film material and its preparation method and application

By using maleic anhydride-styrene-α-methylstyrene ternary copolymer beads as opening agents in degradable copolyester films, combined with aliphatic aromatic copolyester, the problems of difficult film opening and incomplete degradation are solved , achieving easy-to-open, environmentally friendly biodegradation effects, and is suitable for packaging and agricultural mulch films.

CN114437515BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202011132889.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-21
Publication Date
2024-10-15
Estimated Expiration
2040-10-21

AI Technical Summary

Technical Problem

The existing degradable copolyester film is difficult to open after use, resulting in low finished product quality and product qualification rate. Moreover, the degradation products are not entirely water and carbon dioxide, and there is a problem of high haze.

Method used

Maleic anhydride-styrene-α-methylstyrene terpolymer pellets are used as the opening agent, combined with aliphatic aromatic copolyester as the basic resin, and easy opening and controllable biodegradable blow molding are prepared through extrusion granulation and blow molding processes. Plastic film, controlling the mechanical properties and light transmittance of the film.

Benefits of technology

The film achieves easy opening, good mechanical properties and environmentally friendly degradation characteristics. The degradation products are carbon dioxide and water, and is suitable for packaging and agricultural mulching films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114437515B_ABST
    Figure CN114437515B_ABST
Patent Text Reader

Abstract

The present invention relates to an easy-to-open controlled biodegradable blown film material in the field of polymers, as well as a preparation method and application. The easy-to-open controlled biodegradable film material comprises the following components by weight: 100 parts of degradable copolyester; 0.05 to 5 parts of an opening agent, preferably 0.1 to 1.5 parts; the degradable copolyester is a fatty aromatic copolyester; the opening agent is a terpolymer microsphere. The melt index of the degradable copolyester at 190°C and a load of 2.16kg is 0.1 to 10g / 10min. The present invention uses a controlled biodegradable copolyester as a base resin and uses maleic anhydride-styrene-α-methylstyrene terpolymer microspheres as an opening agent to obtain a film material. The film material can be prepared by an upward blowing method to prepare a degradable copolyester blown film, which has the characteristics of simple process, good mechanical properties, easy opening, and biodegradability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymers, and more particularly to an easy-to-open controllable biodegradable blown film material and a preparation method and application thereof. Background Art

[0002] Plastic products have the advantages of strong stability, light weight and low production cost, so they are deeply favored by people. In recent decades, the plastic industry has developed rapidly. The use of a large number of plastic products, especially disposable plastic products, has brought great convenience to human life. However, due to the chemical stability of general plastics (PE, PS, PVC, etc.), they will exist stably in the environment for a long time after being abandoned, resulting in the accumulation of a large amount of plastic waste in the environment, which brings serious harm to the environment, such as white pollution, agricultural white cancer and other problems. With the increasing prominence of environmental problems and the continuous improvement of human environmental protection awareness, the treatment of plastic waste has become the focus of widespread attention in the international community. At present, the main solutions to this problem are incineration, landfill and recycling. The above methods are still commonly used methods for many countries to deal with plastic waste. With the increasing prominence of their own problems, the above methods can no longer meet the requirements of human environmental protection. It is urgent for mankind to fundamentally solve the problem of plastic waste pollution and seek new solutions. After being discarded, degradable plastics can be degraded by certain factors in the environment, so the accumulation of plastic waste in the environment can be reduced, thereby fundamentally solving the problem of plastic waste pollution to the environment. Therefore, the development of degradable plastics has become the ultimate way to solve the problem of plastic waste pollution. For a long time, the base resin of film materials is generally general resins such as PP, PE, PS, etc. However, the films prepared from the above-mentioned polymer materials cannot degrade by themselves after the end of the use cycle, and are easy to cause pollution to the soil, rivers and oceans. In recent years, degradable films have gradually received attention from industry and academia. Poly (butylene succinate-terephthalate) ester (PBST) is a biodegradable polymer compound that can be biodegraded by bacterial fermentation in the natural environment. By regulating the molecular weight of poly (butylene succinate-terephthalate) ester, it can be ensured that it is biodegradable during use.

[0003] In the prior art, when preparing polymer films, especially polyester films, there are a large number of exposed molecular chain ends and migrated oligomer small molecules on the surface, which are polar. When the two layers of film are attached, these exposed molecular chain ends and small molecules will penetrate and entangle with each other, making it difficult to open; after the film is tightly attached, the distance is close, so the van der Waals force between molecules is obvious; during the film blowing process, the film bubble nip roller and the winding process, the film forms a vacuum tight state, which is not easy to separate; with the increase of film making speed, the static electricity accumulation on the film surface increases, showing static electricity adsorption between the films. The above reasons make it difficult to open the degradable copolyester film, which greatly affects the quality of the finished product and the qualified rate of the degradable copolyester film. Usually, in order to overcome the problem of difficulty in opening the polymer film, it is necessary to add corresponding fillers or additives to the film. A lubricant is added to form a lubricant layer between two adjacent layers of the film, which reduces the entanglement of the exposed molecular chain ends of the film and reduces the dynamic and static friction coefficients between the two layers of the film. An antistatic agent is added to eliminate static adsorption; an inorganic opening agent is added to make the surface of the film uneven to increase the distance between the films and reduce the vacuum between the films. However, the degradation products will not be entirely water and carbon dioxide, and the haze will be higher. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention proposes an easy-to-open controlled biodegradable blown film material. Specifically, it relates to an easy-to-open controlled biodegradable blown film material and a preparation method and application. The present invention uses a controlled biodegradable copolyester as a base resin and maleic anhydride-styrene-α-methylstyrene ternary copolymer beads as an opening agent to obtain a film material. The film material can be prepared by an upward blowing method to prepare a degradable copolyester blown film, which has the characteristics of simple process, good mechanical properties, easy opening, and biodegradability.

[0005] One of the purposes of the present invention is to provide an easy-opening controllable biodegradable blown film material, which may include the following components in parts by weight:

[0006] 100 parts of biodegradable copolyester;

[0007] 0.05 to 5 parts of the opening agent, preferably 0.1 to 1.5 parts, more preferably 0.5 to 1 part;

[0008] in,

[0009] The degradable copolyester may be a fatty aromatic copolyester; the fatty aromatic copolyester is obtained by reacting components including monomer a, monomer b, monomer c and monomer d; the fatty aromatic copolyester has a melt index of 0.1 to 10 g / 10 min at 190° C. and a load of 2.16 kg.

[0010] The monomer a may be an aromatic dibasic acid and / or its ester derivative, preferably terephthalic acid and / or dimethyl terephthalate;

[0011] The monomer b may be at least one of a C2-C10 aliphatic diol or a C3-C10 alicyclic diol, preferably 1,3-propylene glycol and / or 1,4-butanediol;

[0012] The monomer c may be a C4-C20 aliphatic dibasic acid and / or its ester derivative, preferably at least one selected from succinic acid, dimethyl succinate, adipic acid or dimethyl adipate;

[0013] The monomer d may be at least one of a polyol having a functionality greater than 2, a polycarboxylic acid having a functionality greater than 2, or an anhydride having a functionality greater than 2, preferably at least one of pyromellitic dianhydride, glycerol, or pentaerythritol.

[0014] As long as a long-chain branched aliphatic aromatic copolyester with a corresponding melt index can be obtained, the content of each monomer can be a conventional amount. Preferably, the amount of the monomer a, monomer b, monomer c and monomer d can be:

[0015] The molar ratio of (a+c):b is 1:(0.8-3); and / or,

[0016] The molar ratio of (a+c):d is (100-2000):1; and / or,

[0017] The molar ratio of a:c is 0:100 to 60:40, preferably 30:100 to 60:40.

[0018] The opening agent is terpolymer microspheres.

[0019] The average particle size of the terpolymer microspheres may be 500 to 1600 nm, preferably 800 to 1600 nm; the terpolymer microspheres may include a copolymer structure of structural unit A, structural unit B and structural unit C; wherein the structural unit A is provided by maleic anhydride; the structural unit B is provided by styrene; the structural unit C is provided by α-methylstyrene;

[0020] Taking the total molar amount of the terpolymer microsphere copolymer structural unit as 100% molar amount, the molar content of the structural unit A is 48-51%, the molar content of the structural unit B is 10-45%, and the molar content of the structural unit C is 10-45%. Preferably, taking the total molar amount of the terpolymer microsphere copolymer structural unit as 100% molar amount, the molar content of the structural unit A is 49-50%, the molar content of the structural unit B is 15-45%, and the molar content of the structural unit C is 10-40%.

[0021] The terpolymer microspheres provided by the present invention contain more maleic anhydride structural units, and the random copolymer obtained thereby has strong polarity while maintaining good compatibility with polyolefins. The terpolymer microspheres are used as an opening agent, and the opening agent is better combined with the copolyester interface, has less effect on mechanical properties and properties such as transmittance and haze, and the degradation products are all carbon dioxide and water.

[0022] The easy-opening controlled biodegradable blown film material may further comprise a lubricant; wherein, based on 100 parts by weight of the degradable copolyester,

[0023] The amount of the lubricant is 0.05 to 5 parts, preferably 0.05 to 2 parts;

[0024] The lubricant is selected from stearates and / or organic carboxylic acid amides, wherein the stearates can be selected from calcium stearate and the like, and the organic carboxylic acid amide can be selected from at least one of erucic acid amide, oleic acid amide, stearic acid stearamide, and N,N'-ethylene bis stearamide, preferably N,N'-ethylene bis stearamide.

[0025] The easy-opening controlled biodegradable blown film material may further comprise a nucleating agent; wherein, based on 100 parts by weight of the degradable copolyester, the amount of the nucleating agent may be 0.1 to 20 parts by weight, preferably 0.5 to 5 parts by weight;

[0026] The nucleating agent may be selected from at least one of hyperbranched polyamide, low density polyethylene, ethylene-methacrylic acid ionomer, or ethylene-butyl acrylate-glycidyl methacrylate terpolymer.

[0027] The easy-opening controlled biodegradable blown film material further comprises an antioxidant; wherein, based on 100 parts by weight of the degradable copolyester, the weight of the antioxidant may be 0.05 to 5 parts by weight, preferably 0.05 to 2 parts by weight.

[0028] The antioxidant may be any antioxidant conventionally used in the art. Preferably, the antioxidant is a hindered phenol antioxidant and a phosphite antioxidant mixed in a mass ratio of 1:3 to 3:1; wherein the hindered phenol antioxidant may be selected from antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; CAS No.: 6683-19-8), 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid; CAS: 27676-62-6) or 330 (1,3,5-trimethyl-2,4,6-tris(3,5-tert-butyl-4-hydroxybenzyl)isocyanuric acid; CAS: 27676-62-6) benzene; CAS: 1709-70-2); the phosphite antioxidant can be selected from at least one of antioxidant 168 (tris [2,4-di-tert-butylphenyl] phosphite; CAS: 31570-04-4), antioxidant 618 (pentaerythritol distearyl diphosphite; CAS: 3806-34-6) or antioxidant 2,2'-ethylene bis (4,6-di-tert-butylbenzene) fluorophosphite; CAS: 118337-09-0).

[0029] The easy-opening controlled biodegradable blown film material may also contain a degradable resin commonly used in the art; wherein, based on 100 parts by weight of the degradable copolyester, the weight of the degradable resin is 2 to 20 parts, preferably 4 to 12 parts; and / or, the degradable resin may be selected from at least one of polycaprolactone, butylene succinate, polyglycolic acid, polylactic acid, polyhydroxyalkanoate (PHA), and polymethyl ethylene carbonate (PPC).

[0030] The second object of the present invention is to provide a method for preparing the easy-opening controllable biodegradable blown film material, which may include the following steps:

[0031] The components including the degradable copolyester, the opening agent, the lubricant, the nucleating agent, the antioxidant and the like are mixed and then extruded and granulated to obtain the easy-opening controllable biodegradable blown film material.

[0032] Alternatively, the degradable copolyester may be mixed with an antioxidant to form granules to obtain a base resin, which is then mixed with other components including an anti-blocking agent and then extruded to form granules.

[0033] Wherein, in the extrusion granulation step, the processing temperature is 150-200° C., preferably 160-190° C., and the screw speed is 250-350 rpm.

[0034] in,

[0035] The preparation method of the degradable copolyester may include the following steps:

[0036] The degradable copolyester can be obtained by reacting components including monomer a, monomer b, monomer c and monomer d under the action of a catalyst to obtain a long-chain branched fatty aromatic copolyester, and then extruding it with an organic peroxide;

[0037] Preferably, the method for preparing the degradable copolyester may include the following steps:

[0038] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, monomer a, monomer b, monomer c and monomer d are mixed for esterification reaction, or the esterification product of monomer a and monomer b and the esterification product of monomer c and monomer d are mixed for co-condensation reaction to obtain long-chain branched aliphatic aromatic copolyester;

[0039] Preferably, the obtained long-chain branched aliphatic aromatic copolyester has a melt index of 5-100 g / 10 min at 190° C. and 2.16 kg load;

[0040] 2) Extruding the long-chain branched aliphatic aromatic copolyester prepared in step 1) and an organic peroxide to obtain the degradable copolyester.

[0041] in,

[0042] The monomer a is an aromatic dibasic acid or an ester derivative thereof; the monomer b is a C2-C 10 Aliphatic diols or C3-C 10 One or more of alicyclic diols; the monomer c is C4-C 20 The monomer d is one or more of a polyol with a functionality greater than 2, a polycarboxylic acid with a functionality greater than 2, or an anhydride with a functionality greater than 2;

[0043] Preferably, the monomer a is terephthalic acid or dimethyl terephthalate; the monomer b is 1,3-propylene glycol or 1,4-butanediol; the monomer c is selected from succinic acid, dimethyl succinate, adipic acid or dimethyl adipate; and the monomer d is pyromellitic anhydride, glycerol or pentaerythritol.

[0044] In order to obtain a long-chain branched aliphatic aromatic copolyester with better performance, preferably, the amounts of monomer a, monomer b, monomer c and monomer d are as follows: the molar ratio of (a+c):b is 1:(0.8-3), the molar ratio of (a+c):d is 100-2000:1, and the molar ratio of a:c is 0:100-60:40, wherein a+c refers to the total amount of monomer a and monomer c.

[0045] The catalyst contains at least one of a first catalyst, a second catalyst and a third catalyst;

[0046] The first catalyst may be selected from at least one of an oxide of M, M(OR1)n and M(OOCR2)m, wherein M is titanium, antimony or zinc, n and m are each independently the valence state of M, and R1 is C1-C 10 Alkyl, R2 is C1-C 20 Preferably, the first catalyst may be selected from at least one of alkoxytitanium, antimony acetate, zinc acetate, zinc oxide, antimony oxide and titanium oxide; More preferably, the first catalyst may be selected from at least one of tetrabutyl titanate (Ti(OC4H9)4), isopropoxytitanium, titanium dioxide, antimony trioxide, antimony acetate and zinc acetate;

[0047] and / or,

[0048] The second catalyst may be a compound of RE(R3)3, wherein RE is a rare earth metal element, R3 is selected from at least one of halogen, alkoxy, aryloxy, acetylacetonato and R4COO-, and R4 is C1-C 30 Preferably, RE is selected from at least one of lanthanum, cerium, praseodymium, neodymium, terbium, ytterbium, dysprosium, samarium or scandium;

[0049] The halogen may be chlorine or bromine, the alkoxy may be a C3-C6 alkoxy, the aryloxy may be an aryloxy including at least one benzene ring and / or naphthalene ring, R4 may be a C1-C 20 The alkyl group;

[0050] In a further preferred embodiment, RE is selected from lanthanum, cerium, praseodymium, neodymium or scandium, the halogen is chlorine or bromine, the alkyl in the alkoxy is at least one of isopropyl, n-butyl or isopentyl, the aryl in the aryloxy is at least one of 2,6-di-tert-butyl-4-methylphenyl or 4-butylphenyl, and R4 is C3-C 18 At least one of the alkyl groups;

[0051] In a more preferred case, the second catalyst may be at least one of lanthanum acetylacetonate, neodymium acetylacetonate, neodymium isopropoxide, lanthanum isopropoxide, scandium isopropoxide, lanthanum stearate, neodymium stearate, lanthanum chloride, tris(2,6-di-tert-butyl-4-methylphenoxy)lanthanum and hydrates thereof;

[0052] and / or,

[0053] The third catalyst may be at least one organic tin compound; preferably, the third catalyst may be selected from dibutyltin oxide, methylphenyltin oxide, tetraethyltin, hexaethyltin oxide, hexacyclohexyl ditin oxide, didodecyltin oxide, triethylhydroxytin, triphenylhydroxytin, triisobutyltin acetate, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin sulfide, butyl hydroxytin oxide, methylstannic acid, ethylstannic acid and butylstannic acid; further preferably, the third catalyst may be selected from a mixture of at least two of dibutyltin oxide, tetraethyltin, triphenylhydroxytin, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin sulfide, butyl hydroxytin oxide, methylstannic acid, ethylstannic acid and butylstannic acid; in this case, the total molar amount of the third catalyst may be 100%. The content of each component of the third catalyst may be 10 to 90 mol %, preferably 30 to 70 mol %.

[0054] The catalyst of the present invention can be selected in conventional dosage in the art. Preferably, the molar ratio of the total dosage of the catalyst to the monomer (a+c) can be 1:(1000-20000); preferably 1:(1000-10000). And / or,

[0055] The molar ratio of the first catalyst: the second catalyst: the third catalyst may be (0.1-20): (0.1-10): 1, preferably (0.1-10): (0.1-10): 1.

[0056] The organic peroxide may be selected from organic peroxides having a half-life of 0.2 to 10 min within the processing temperature range, preferably a half-life of 0.2 to 2 min;

[0057] Further preferably, the organic peroxide may be selected from at least one of alkyl peroxides, acyl peroxides and peroxyesters;

[0058] Preferably, the organic peroxide can be selected from at least one of 2,5-bis(tert-amyl peroxy)-2,5-dimethylhexane, 2,5-bis(tert-butyl peroxy)-2,5-dimethylhexane, 3,6-bis(tert-butyl peroxy)-3,6-dimethyloctane, 2,7-bis(tert-butyl peroxy)-2,7-dimethyloctane, 8,11-bis(tert-butyl peroxy)-8,11-dimethyloctadecane or a mixture thereof, bis(alkyl peroxy)benzene, and bis(alkyl peroxy)alkyne;

[0059] Wherein, the bis(alkylperoxide)benzene may be selected from α,α'-(tert-amylperoxide-isopropyl)benzene, α,α'-bis(tert-butylperoxide-isopropyl)benzene or a mixture thereof;

[0060] The bis(alkylperoxy)alkyne may be selected from 2,7-dimethyl-2,7-di(tert-butylperoxy)-octanediyne-3,5,2,7-dimethyl-2,7-di(peroxyethyl carbonate)-octanediyne-3,5,3,6-dimethyl-3,6-di(peroxyethyl carbonate) At least one of octyne-4,3,6-dimethyl-3,6-di(tert-butyl-peroxy)octyne-4,2,5-dimethyl-2,5-di(peroxy-n-propyl-carbonate)hexyne-3,2,5-dimethyl-2,5-di(peroxy-isobutyl carbonate)hexyne-3,2,5-dimethyl-2,5-di(peroxyethyl monocarbonate)hexyne-3,2,5-dimethyl-2,5-di((α-cumylperoxy)hexyne-3,2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3.

[0061] The amount of the organic peroxide in the present invention can be a conventional amount. For example, the amount of the organic peroxide can be 0.01 to 5 wt %, preferably 0.01 to 1 wt %, of the amount of the long-chain branched aliphatic aromatic copolyester.

[0062] In step 1),

[0063] In the present invention, the conditions of the esterification reaction and the polycondensation reaction can be conventionally selected according to the prior art. For example, the esterification reaction temperature can be 150-220° C.; the polycondensation reaction conditions can include: a temperature of 250-270° C. and a time of 2-3 hours.

[0064] The long-chain branched aliphatic aromatic copolyester prepared in step 1) may have a melt index of 5 to 100 g / 10 min at 190° C. and a load of 2.16 kg;

[0065] In step 2), the extrusion temperature may be 150-200°C, preferably 160-180°C.

[0066] Preferably, the copolyester prepared in step 2) has a melt index of 0.1-10 g / 10 min at 190° C. and a load of 2.16 kg.

[0067] The degradable copolyester can be obtained according to the above description or according to the record in CN201910878788.9. The degradable copolyester of the present invention adopts a long-chain branched aliphatic aromatic copolyester as the main material, which is subjected to extrusion chain extension and viscosity enhancement to further increase the length of the branch chain, while reducing the melt index and increasing its melt strength, and at the same time, with the corresponding processing aids, a high-strength film product is prepared, which can be completely degraded into small molecular products such as carbon dioxide and water under natural or composting conditions.

[0068] The method for preparing an easily-openable and controllably biodegradable film material of the present invention may include adding maleic anhydride-α-methylstyrene-styrene ternary copolymer beads and blending and extruding them before the extrusion granulation, which can achieve a better synergistic effect of opening and high mechanical strength.

[0069] In the easy-opening controllable biodegradable film material of the present invention, the degradable copolyester and the antioxidant may be mixed and granulated first, and then the above-mentioned compound and other components in the composition of the present invention may be mixed; degradable resins such as polycaprolactone and butylene succinate may also be added for extrusion granulation. The degradable copolyester film that meets the purpose of the present invention can be prepared.

[0070] The preparation method of the opening agent may include the following steps:

[0071] In an inert atmosphere, components including polymerization monomers and initiators are dissolved in a reaction medium to form a homogeneous solution; the homogeneous solution is polymerized to obtain a copolymer emulsion suspension, and then centrifuged to obtain the terpolymer microspheres;

[0072] The polymerizable monomers include maleic anhydride, styrene and α-methylstyrene. Based on the total amount of the polymerizable monomers, the molar content of maleic anhydride is 48-51% (preferably 49-50%); and the molar ratio of styrene to α-methylstyrene is 9:1-1:9 (preferably 6:1-1:6).

[0073] Based on the total weight of the homogeneous solution, the mass concentration of the polymerizable monomer is 4 to 22 wt %, preferably 15 to 22 wt %.

[0074] The initiator may be an organic peroxide and / or an azo compound. The organic peroxide may be selected from at least one of dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate; the azo compound may be selected from azobisisobutyronitrile and / or azobisisoheptylonitrile.

[0075] Based on the total weight of the homogeneous solution, the amount of the initiator used is 0.4 to 4 wt %, preferably 0.5 to 3.6 wt %, of the total weight of the homogeneous solution.

[0076] According to the present invention, the reaction medium is an organic acid alkyl ester.

[0077] In the present invention, an organic acid alkyl ester is selected as a reaction medium, which can cooperate with the specific amount of maleic anhydride, α-methylstyrene and styrene described in the present invention to achieve a self-stabilizing precipitation polymerization reaction of maleic acid, α-methylstyrene and styrene. No stabilizer or co-stabilizer needs to be added to the polymerization reaction system, and the system has a self-stabilizing dispersion effect. The surface of the obtained copolymer microspheres is clean and pollution-free.

[0078] According to the present invention, the general formula of the organic acid alkyl ester is R1COOR2, wherein R1 is selected from H, C 1-4 At least one of an alkyl group, a phenyl group and a benzyl group, R2 is C 1-10 Preferably, R1 is C 1-4 alkyl and / or phenyl, R2 is C 1-7 of alkyl.

[0079] According to the present invention, the reaction medium can be selected from at least one of ethyl formate, propyl formate, isobutyl formate, pentyl formate, ethyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, pentyl acetate, isoamyl acetate, benzyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate, isoamyl butyrate, ethyl isovalerate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate and ethyl phenylacetate.

[0080] In the present invention, the polymerization reaction is carried out in an inert atmosphere, and the inert atmosphere can be provided by conventional inert gases in the prior art, such as nitrogen.

[0081] According to the present invention, the conditions of the polymerization reaction include: a polymerization temperature of 60 to 95° C., preferably 65 to 76° C.; and a polymerization time of 2 to 24 hours, preferably 4 to 8 hours.

[0082] The reactor or reaction equipment in the preparation method of the present invention are common reactors or reaction equipment in the prior art.

[0083] In the present invention, maleic anhydride, alpha-methylstyrene and styrene are copolymerized in the presence of a reaction medium in a copolymerization manner according to the method defined in the present invention, and the amount of maleic anhydride and the molar ratio of styrene to alpha-methylstyrene in the polymerization monomers are regulated to achieve self-stabilizing dispersion of the polymerization system. The prepared polymer is in the form of microspheres with excellent uniformity, and no additives such as stabilizers and precipitants need to be added during the polymerization process. The polymer has a self-stabilizing dispersion effect, and the obtained copolymer microspheres have the characteristics of uniform particle size and clean surface, good dispersibility in the medium, and no aggregation occurs.

[0084] In the present invention, in order to obtain copolymer microspheres with uniform particles and excellent morphology, the inventors studied the feed ratio between maleic anhydride, α-methylstyrene and styrene during the polymerization process. The study shows that when the feed amount of each polymerization monomer meets the range specified by the present invention, copolymer microspheres with uniform particles, excellent particle morphology and clean particle surface can be obtained.

[0085] The terpolymer microsphere opening agent of the present invention can be obtained according to the above description or with reference to the records in CN201911018149.1. In order to achieve self-stabilization of the polymerization system and obtain copolymer microspheres with particle sizes and clean and pollution-free, the inventors studied the conditions of the polymerization reaction. Studies have shown that when the polymerization temperature is 60 to 95°C and the polymerization time is 2 to 24h, the polymerization system forms a stable self-stabilizing system, in which the polymerization monomers maleic anhydride, α-methylstyrene and styrene are polymerized to form microspheres, and the microspheres do not aggregate in the medium and have good dispersibility.

[0086] The third object of the present invention is to provide a film made of the easy-opening controllable biodegradable blown film material. The film meets environmental protection requirements, is controllable degradable, easy to open, has low production cost and is suitable for large-scale production.

[0087] According to the present invention, the thickness of the film can be adjusted according to the needs and specific processes. Preferably, the thickness of the film can be 5 to 100 μm, preferably 10 to 20 μm;

[0088] and / or,

[0089] The tensile breaking stress of the film is greater than 18 MPa, preferably greater than 25 MPa, for example, it can be 25-100 MPa.

[0090] Preferably, the longitudinal tensile strength of the degradable copolyester blown film is above 18 MPa, and the transverse tensile strength is above 16 MPa; preferably, the longitudinal tensile strength is above 24 MPa, and the transverse tensile strength is above 20 MPa.

[0091] Preferably, the longitudinal elongation at break of the degradable copolyester blown film is greater than 250%, and the transverse elongation at break is greater than 300%; preferably, the longitudinal elongation at break is greater than 300%, and the transverse elongation at break is greater than 350%.

[0092] Preferably, the light transmittance of the degradable copolyester blown film is above 89%.

[0093] The fourth object of the present invention is to provide a method for preparing a film made of the easy-opening controllable biodegradable blown film material. The preparation method may include the following steps: blowing the easy-opening controllable biodegradable blown film material into a film;

[0094] Preferably,

[0095] The film blowing temperature may be 150-210°C, preferably 175-195°C; and / or,

[0096] In the film blowing process, the blow ratio may be 1.5 to 3, preferably 2 to 2.5.

[0097] The method for preparing a film made of the easy-opening controllable biodegradable blown film material of the present invention, specifically the method for preparing a degradable copolyester blown film, may include:

[0098] I) mixing the degradable copolyester and the antioxidant and granulating them, preferably the weight ratio of the degradable copolyester to the antioxidant is 100:(0.05-0.5), to obtain a base resin;

[0099] II) (1) dissolving a polymerization monomer and an initiator in a reaction medium in an inert atmosphere to form a homogeneous solution;

[0100] (2) subjecting the homogeneous solution to polymerization to obtain a copolymer emulsion suspension, and then centrifuging to obtain the terpolymer microspheres;

[0101] The polymerizable monomers are maleic anhydride, styrene and α-methylstyrene; based on the total amount of the polymerizable monomers, the molar content of maleic anhydride is 48-51%; and the molar ratio of styrene to α-methylstyrene is 9:1-1:9.

[0102] III) mixing the base resin obtained in step I) and the compound obtained in step II), adding additives such as a nucleating agent and a lubricant, and extruding and granulating the mixture, and then blowing the obtained granules into films.

[0103] Preferably, the granules are extruded by a twin-screw extruder and then blown into a film by a film blowing machine.

[0104] Preferably, the extrusion temperature is 150-200° C., preferably 170-190° C.; the screw speed is 250-350 rpm.

[0105] The extrusion temperature refers to the extrusion temperature set by the extrusion equipment, such as an extruder. The film blowing temperature refers to the film outlet temperature of the film blowing equipment, such as a film blowing machine.

[0106] According to the present invention, the film blowing machine used can be a downward blowing water-cooled type, a horizontal blowing air-cooled type, or a traditional upward blowing air-cooled biodegradable copolyester film blowing machine unit.

[0107] A fifth object of the present invention is to provide the application of the film in agricultural mulch films and packaging bag films.

[0108] The film prepared by using the easy-opening controllable biodegradable film material described in this method is a degradable copolyester blown film, which has the advantages of biodegradability and easy opening, and can be used in packaging and agricultural films and other occasions where there are high requirements for the biodegradability of plastic products and opening.

[0109] Compared with the prior art, the present invention has the following beneficial effects:

[0110] 1) The degradable copolyester composition provided by the present invention has good mechanical properties, and is therefore suitable for use as an excellent material in the fields of packaging, protective films, agricultural greenhouse films, and ground films. The preparation method of the degradable copolyester composition provided by the present invention is simple, effective, and easy to operate.

[0111] 2) The manufactured degradable blown film has a controllable degradation structure and can be degraded in landfills without causing secondary pollution, thus meeting the requirements of a circular economy. BRIEF DESCRIPTION OF THE DRAWINGS

[0112] Figure 1 This is the infrared spectrum (FI-IR spectrum) of the ternary copolymer microsphere SYXQ101 described in Example 1 of the present application. 1785cm -1 、1850cm -1 It is the characteristic absorption peak of anhydride group, 709cm -1 It is the special absorption peak of benzene ring, 1020-1300cm -1 It is the characteristic peak of CN group. Based on this, it can be determined that the polymer is maleic anhydride / styrene / α-methylstyrene copolymer.

[0113] Figure 2 This is a scanning electron microscope image (SEM image) of the ternary copolymer microspheres SYXQ101 described in Example 1 of the present application. It can be seen from the image that the particles of the copolymer microspheres are uniform and the particle surface is clean and not contaminated. DETAILED DESCRIPTION

[0114] The present invention will be further described below in conjunction with the embodiments, but the present invention is not limited by these embodiments.

[0115] The present invention is further described with reference to the following examples, but it should be construed that the present invention is by no means limited to these examples.

[0116] Other raw materials used in the examples and comparative examples are all commercially available.

[0117] The testing methods of the relevant data in the following examples and comparative examples are as follows:

[0118] The morphology and size of the terpolymer microspheres were observed and measured using scanning electron microscopy (SEM);

[0119] The infrared spectra of copolymers were tested by FI-IR;

[0120] The content of each structural unit in the copolymer is 1 H NMR was tested by 1 The content of each structural unit was calculated from the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in H NMR.

[0121] The molecular weight and molecular weight distribution of the polymer were determined by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as solvent on a Waters-208 instrument (with a Waters 2410 RI detector, a flow rate of 1.5 mL / min, and 30° C.) and the molecular weight was calibrated with a styrene standard.

[0122] The crystallization temperature (Tc) and melting temperature (Tm) of the polymers were determined by differential scanning calorimetry (DSC). Each sample was heated from -100°C to 250°C in two heating scans on a PerkinElmer Pyris 1 instrument at a heating rate of 20°C / min.

[0123] Determination of melt index (MI): The melt flow rate of the polymer was determined using a CS-127 melt indexer manufactured by Scientific Instruments, Inc. at 190°C and a load of 2.16 kg in accordance with ISO1133-2005 "Determination of mass flow rate and volume flow rate of thermoplastic melts" standard.

[0124] Determination of light transmittance and haze: Determine according to the description in national standard GB / T 2410-2008.

[0125] Examples 1-6 are used to illustrate the degradable copolyester blown film with good light transmittance and easy opening of the present invention and the preparation method thereof.

[0126] Example 1

[0127] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0128] (1) Preparation of ternary copolymer microspheres SYXQ101:

[0129] 11g maleic anhydride, 0.6g azobisisobutyronitrile, 10.62g α-methylstyrene, 1.04g styrene and 87.8g isoamyl acetate were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into a 60°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 11.04g of polymer solid A1, corresponding to a polymer yield of 51.4%. The particle size of the polymer microspheres was 1200 nanometers. Among them, the molar ratio of styrene to α-methylstyrene was 1:9.

[0130] The polymer microspheres A1 were subjected to 1H NMR measurement, and the molar content of maleic anhydride structural units was 50%, the molar content of styrene structural units was 10%, and the molar content of α-methylstyrene structural units was 40% based on the total molar amount of each structural unit in the polymer.

[0131] (2) Preparation of degradable copolyester composition 101:

[0132] 1) Under the action of a catalyst, 423.8 g (2.55 mol) of terephthalic acid (PTA) of monomer a, 650 g (7.21 mol) of 1,4-butanediol (BDO) of monomer b, 330 g (2.79 mol) of succinic acid (SA) of monomer c and 1 g (0.01 mol) of propylene glycol of monomer d were mixed for esterification to obtain a long-chain branched aliphatic aromatic copolyester having a melt index of 23 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.245 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.31 g of lanthanum stearate, 0.1 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), and 0.14 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company);

[0133] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 2.5 g of 3,6-bis(tert-butylperoxy)-3,6-dimethyloctane are subjected to extrusion reaction at 170° C. in an extruder to prepare a copolyester, wherein the melt index of the copolyester prepared is 1.9 g / 10 min at 190° C. and a load of 2.16 kg;

[0134] (3) Preparation of Blown Film 101:

[0135] 500 g of the obtained copolyester was mixed with 1 g of antioxidant 1010, 2 g of antioxidant 168, 1.5 g of lubricant N,N'-ethylene bis stearamide, 4 g of anti-blocking agent SYXQ101, and 25 g of nucleating agent DuPont Elvaloy 4170 resin, and added into a twin-screw extruder for melt extrusion and granulation at 170° C. to obtain a blown film material;

[0136] (4) The film blowing material is blown on a film blowing machine with a die temperature of 180° C. and a blowing ratio of 2.3:1 to obtain a film with a thickness of 10 μm.

[0137] The prepared film was subjected to performance tests, and the test results of its optical properties, thermal properties and barrier properties are shown in Table 1, and its mechanical properties are shown in Table 2.

[0138] Example 2

[0139] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0140] (1) Preparation of ternary copolymer microspheres SYXQ102

[0141] 10g maleic anhydride, 0.89g azobisisobutyronitrile, 9.44g α-methylstyrene, 2.08g styrene and 87.8g butyl butyrate were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into a 70°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 11.72g of polymer solid A2, corresponding to a polymer yield of 55.0%. The particle size of the polymer microspheres was 1500 nanometers. Among them, the molar ratio of styrene to α-methylstyrene was 2:8.

[0142] The polymer microspheres A2 were 1 H NMR measurement showed that based on the total molar amount of each structural unit in the polymer, the molar content of maleic anhydride structural unit was 48%, the molar content of styrene structural unit was 12%, and the molar content of α-methylstyrene structural unit was 40%.

[0143] (2) Preparation of biodegradable copolyester 102

[0144] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, 423.8 g (2.55 mol) of terephthalic acid, 570.8 g (7.5 mol) of 1,3-propylene glycol, 438.4 g (3 mol) of dimethyl succinate, and 1 g (0.0046 mol) of pyromellitic anhydride were mixed for esterification reaction. The obtained long-chain branched aliphatic aromatic copolyester had a melt index of 15 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.245 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.31 g of lanthanum stearate, 0.1 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), and 0.14 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company);

[0145] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 2.5 g of 3,6-bis(tert-butylperoxy)-3,6-dimethyloctane are subjected to extrusion reaction at 170° C. in an extruder to prepare a copolyester, wherein the melt index of the copolyester prepared is 2.0 g / 10 min at 190° C. and a load of 2.16 kg;

[0146] (3) Preparation of Blown Film 102

[0147] 500 g of the above copolyester was mixed with 1 g of antioxidant 31141 g, 2 g of antioxidant 168, 2.25 g of lubricant oleic acid amide, 1.5 g of anti-blocking agent SYXQ102, and 15 g of nucleating agent DuPont Surlyn 8920 resin, and added into a twin-screw extruder for melt extrusion and granulation at 170° C. to obtain a blown film material;

[0148] (4) The film blowing material is blown on a film blowing machine with a die temperature of 185° C. and a blowing ratio of 2.2:1 to obtain a film with a thickness of 10 μm.

[0149] The prepared film was subjected to performance tests, and the test results of its optical properties, thermal properties and barrier properties are shown in Table 1, and its mechanical properties are shown in Table 2.

[0150] Example 3

[0151] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0152] (1) Preparation of ternary copolymer microspheres SYXQ103

[0153] 10.2g maleic anhydride, 0.7g azobisisobutyronitrile, 8.26g α-methylstyrene, 3.12g styrene and 80g butyl benzoate were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into an 80°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 16.38g of polymer solid A3, corresponding to a polymer yield of 77.3%. The particle size of the polymer was 1600 nanometers. The molar ratio of styrene to α-methylstyrene was 3:7.

[0154] The polymer microsphere A3 was subjected to 1H NMR measurement, and the molar content of maleic anhydride structural units was 51%, the molar content of styrene structural units was 15%, and the molar content of α-methylstyrene structural units was 34% based on the total molar amount of each structural unit in the polymer.

[0155] (2) Preparation of biodegradable copolyester 103

[0156] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, 679.6 g (3.5 mol) of dimethyl terephthalate (a), 570.8 g (7.5 mol) of 1,3-propylene glycol (b), 657.6 g (4.5 mol) of adipic acid (c) and 0.7 g (0.005 mol) of pentaerythritol (d) were mixed for esterification reaction, and the obtained long-chain branched aliphatic aromatic copolyester had a melt index of 40 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.245 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.31 g of lanthanum stearate, 0.1 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), and 0.14 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company);

[0157] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 2.5 g of 3,6-bis(tert-butylperoxy)-3,6-dimethyloctane are subjected to extrusion reaction in an extruder at 170° C. to prepare a copolyester, wherein the melt index of the copolyester prepared is 2.6 g / 10 min at 190° C. and a load of 2.16 kg;

[0158] (3) Preparation of Blown Film 103

[0159] 500 g of the above copolyester was mixed with 3301 g of antioxidant, 6182 g of antioxidant, 2 g of stearic acid stearamide, 2.25 g of SYXQ103, and 25 g of Elvaloy 4170 resin, and added into a twin-screw extruder for melt extrusion and granulation at 170° C. to obtain a blown film material;

[0160] 4) The film blowing material was blown on a film blowing machine with a die temperature of 180° C. and a blowing ratio of 2.2:1 to obtain a film with a thickness of 10 μm.

[0161] The prepared film was subjected to performance tests, and the test results of its optical properties, thermal properties and barrier properties are shown in Table 1, and its mechanical properties are shown in Table 2.

[0162] Example 4

[0163] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0164] (1) Preparation of ternary copolymer microspheres SYXQ104:

[0165] 9.6g of maleic anhydride, 0.85g of azobisisobutyronitrile, 7.08g of α-methylstyrene, 4.16g of styrene and 85.8g of butyl acetate were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into a 65°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 16.63g of polymer solid A4, corresponding to a polymer yield of 79.0%. The particle size of the polymer microspheres was 1500 nanometers. Among them, the molar ratio of styrene to α-methylstyrene was 4:6.

[0166] The polymer microsphere A4 was subjected to 1H NMR measurement, and the molar content of maleic anhydride structural units was 49%, the molar content of styrene structural units was 20%, and the molar content of α-methylstyrene structural units was 31% based on the total molar amount of each structural unit in the polymer.

[0167] (2) Preparation of degradable copolyester 104:

[0168] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, 423.8 g (2.55 mol) of terephthalic acid (PTA) of monomer a, 650 g (7.21 mol) of 1,4-butanediol (BDO) of monomer b, 330 g (2.79 mol) of succinic acid (SA) of monomer c and 1 g (0.01 mol) of propylene glycol of monomer d were mixed for esterification reaction, and the obtained long-chain branched aliphatic aromatic copolyester had a melt index of 40 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.174 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.071 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), 0.099 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company) and 0.22 g of lanthanum stearate;

[0169] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 5 g of 2,7-bis(tert-butylperoxy)-2,7-dimethyloctane are subjected to extrusion reaction in an extruder at 180° C. to prepare a copolyester, wherein the melt index of the copolyester prepared is 2.3 g / 10 min at 190° C. and a load of 2.16 kg;

[0170] (3) Preparation of blown film 104;

[0171] 1) 500 g of the above-mentioned degradable copolyester 104 was mixed with 3301 g of antioxidant, 2.5 g of antioxidant 2,2'-ethylenebis(4,6-di-tert-butylbenzene)fluorophosphite, 2 g of lubricant N,N'-ethylenebisstearamide, 2.25 g of opening agent SYXQ104, 15 g of nucleating agent DuPont Surlyn8920 resin, and 50 g of polycaprolactone, and added into a twin-screw extruder for melt extrusion and granulation at 180° C. to obtain a blown film material;

[0172] 2) The film blowing material was blown on a film blowing machine with a die temperature of 190° C. and a blowing ratio of 2.5:1 to obtain a film with a thickness of 10 μm.

[0173] The prepared film was subjected to performance tests, and the test results of its optical properties, thermal properties and barrier properties are shown in Table 1, and its mechanical properties are shown in Table 2.

[0174] Example 5

[0175] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0176] (1) Ternary copolymer microspheres The polymer microspheres SYXQ104 prepared in Example 4 were taken.

[0177] (2) Preparation of degradable copolyester 105:

[0178] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, 423.8 g (2.55 mol) of terephthalic acid, 570.8 g (7.5 mol) of 1,3-propylene glycol, 438.4 g (3 mol) of dimethyl succinate, and 1 g (0.0046 mol) of pyromellitic anhydride were mixed for esterification reaction. The obtained long-chain branched aliphatic aromatic copolyester had a melt index of 15 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.245 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.31 g of lanthanum stearate, 0.1 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), and 0.14 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company);

[0179] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 0.5 g of dibenzoyl peroxide are subjected to extrusion reaction at 160° C. in an extruder to prepare a copolyester, wherein the melt index of the copolyester prepared is 1.5 g / 10 min at 190° C. and a load of 2.16 kg;

[0180] (3) Preparation of Blown Film 105

[0181] 500g of copolyester 105, 1g of antioxidant 1010, 1g of antioxidant 618, 2.25g of lubricant erucamide, 3g of anti-blocking agent SYXQ105, 10g of Elvaloy 4170 resin, and 50g of butylene succinate were added into a twin-screw extruder for melt extrusion and granulation at 160°C to obtain a blown film material;

[0182] (4) The film blowing material is blown on a film blowing machine with a die temperature of 185° C. and a blowing ratio of 2:1 to obtain a film with a thickness of 10 μm.

[0183] The prepared film was subjected to performance tests, and the test results of its optical properties, thermal properties and barrier properties are shown in Table 1, and its mechanical properties are shown in Table 2.

[0184] Example 6

[0185] This example is used to illustrate the degradable copolyester composition, ternary copolymer microspheres and degradable copolyester blown film provided by the present invention.

[0186] (1) Preparation of ternary copolymer microspheres SYXQ106:

[0187] 9.6g maleic anhydride, 0.69g azobisisobutyronitrile, 4.72g α-methylstyrene, 6.24g styrene and 86.8g isoamyl acetate were added to a 500mL three-necked flask. After the materials were mixed evenly, nitrogen was passed through for 20 minutes, and the three-necked flask was moved into a 75°C water bath to react for 3 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 16.65g of polymer solid A6, corresponding to a polymer yield of 75%. The maleic anhydride content in the polymer was 51%. The particle size of the polymer microspheres was 1400 nanometers. Among them, the molar ratio of styrene to α-methylstyrene was 6:4.

[0188] The polymer microsphere A6 was subjected to 1H NMR measurement, and the molar content of maleic anhydride structural units was 51%, the molar content of styrene structural units was 27%, and the molar content of α-methylstyrene structural units was 22% based on the total molar amount of each structural unit in the polymer.

[0189] (2) Preparation of degradable copolyester 106:

[0190] 1) Preparation of long-chain branched aliphatic aromatic copolyester: Under the action of a catalyst, 423.8 g (2.55 mol) of terephthalic acid (PTA) of monomer a, 650 g (7.21 mol) of 1,4-butanediol (BDO) of monomer b, 330 g (2.79 mol) of succinic acid (SA) of monomer c and 1 g (0.01 mol) of propylene glycol of monomer d were mixed for esterification reaction, and the obtained long-chain branched aliphatic aromatic copolyester had a melt index of 25 g / 10 min at 190° C. and a load of 2.16 kg; the catalyst contained 0.245 g of tetrabutyl titanate (purchased from Beijing Chemical Reagent Company), 0.31 g of lanthanum stearate, 0.1 g of dibutyltin oxide (purchased from Beijing Chemical Plant No. 3), and 0.14 g of triphenylhydroxytin (purchased from Beijing Chemical Reagent Company);

[0191] 2) 500 g of the long-chain branched aliphatic aromatic copolyester prepared in step 1) and 2.5 g of dibenzoyl peroxide were subjected to extrusion reaction at 170° C. in an extruder to prepare a copolyester, wherein the melt index of the copolyester prepared at 190° C. and a load of 2.16 kg was 1.8 g / 10 min;

[0192] (3) Preparation of blown film 106:

[0193] 500 g of the copolyester obtained in step 2) was mixed with 1.5 g of antioxidant 3114, 3 g of 2,2'-ethylenebis(4,6-di-tert-butylbenzene)fluorophosphite, 1 g of lubricant stearamide, 1 g of opening agent SYXQ106, 5 g of Elvaloy4170 resin, and 25 g of polycaprolactone PCL, and added into a twin-screw extruder for melt extrusion and granulation at 170° C. to obtain a blown film material;

[0194] The film blowing material was blown on a film blowing machine with a die temperature of 175° C. and a blowing ratio of 2.5:1 to obtain a film with a thickness of 10 μm.

[0195] Comparative Example 1

[0196] This comparative example is used to illustrate the reference biodegradable copolyester raw material, terpolymer pellets and blown film.

[0197] The degradable copolyester raw material is the same as that of Example 101, but without the chain extension modification in step 2), to obtain copolyester 107. The ternary copolymer pellet is SYXQ101.

[0198] The preparation of the blown film is the same as in Example 101:

[0199] After multiple attempts at blow molding, the film bubble ruptured and the film could not be formed.

[0200] Comparative Example 2

[0201] The same procedures as in Example 1 were followed except that the anti-blocking agent was changed to talcum powder produced by Dalian Fuji Mining Company and had a particle size distribution of 2-5 μm.

[0202] Comparative Example 3

[0203] Except that the degradable copolyester was changed to commercially available PBAT (polybutylene adipate / terephthalate), the other steps were the same as those in Example 1.

[0204] Table 1

[0205] <![CDATA[Density / g.cm -3 > Light transmittance / % Haze / % Melting point / ℃ odor Example 1 1.25 89 13 127 ○ Example 2 1.25 92 14 126 ○ Example 3 1.24 89 12 122 ○ Example 4 1.25 90 15 124 ○ Example 5 1.24 89 13 127 × Example 6 1.25 91 16 128 × Comparative Example 1 1.24 - - - ○ Comparative Example 2 1.25 82 40 126 ○ Comparative Example 3 1.25 87 41 125 ○

[0206] Note: Good smell: ○; Smell: ×

[0207] Table 2

[0208]

[0209] ○ The pores are dense and uniform, × The pores are sparse and uneven

[0210] It can be seen from the data in Table 1 and Table 2 that when the terpolymer microspheres provided by the present invention are added to the degradable copolyester and blown film is performed, the obtained film has excellent opening performance and better mechanical properties.

[0211] As can be seen from Table 1, compared with Comparative Example 2, Examples 1 to 6 have better light transmittance and haze, lower opening force and water permeability. Among them, Example 4 adds polycaprolactone and has better mechanical properties. The melt strength of PBST without chain extension is poor and cannot be blown to obtain a film. Examples 5 and 6 use traditional dibenzoyl peroxide, which has a strong odor. Although PCL and PBS are added, the mechanical properties are low.

[0212] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. An easy-opening controlled biodegradable blown film material, comprising the following components in parts by weight: 100 parts of biodegradable copolyester; 0.05-5 parts of opening agent; The degradable copolyester is an aliphatic aromatic copolyester; The opening agent is terpolymer microspheres; The terpolymer microspheres comprise a copolymer structure of structural unit A, structural unit B and structural unit C; wherein, The structural unit A is provided by maleic anhydride; the structural unit B is provided by styrene; the structural unit C is provided by α-methylstyrene; Taking the total molar amount of the terpolymer microspheres as 100% molar amount, the molar content of the structural unit A is 48-51%; the molar content of the structural unit B is 10-45%; and the molar content of the structural unit C is 10-45%.

2. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that: The melt index of the degradable copolyester at 190° C. and 2.16 kg load is 0.1 to 10 g / 10 min.

3. The easy-opening controlled biodegradable blown film material according to claim 2, characterized in that: The degradable copolyester is obtained by reacting components including monomer a, monomer b, monomer c and monomer d; in, The monomer a is an aromatic dibasic acid and / or its ester derivative; The monomer b is at least one of a C2-C10 aliphatic diol or a C3-C10 alicyclic diol; The monomer c is a C4-C20 aliphatic dibasic acid and / or its ester derivative; The monomer d is at least one of a polyol having a functionality greater than 2, a polycarboxylic acid having a functionality greater than 2, or an acid anhydride having a functionality greater than 2.

4. The easy-opening controlled biodegradable blown film material according to claim 3, characterized in that: The amounts of monomer a, monomer b, monomer c and monomer d are as follows: The molar ratio of (a+c):b is 1:(0.8-3); and / or, The molar ratio of (a+c):d is (100-2000):1; and / or, The molar ratio of a:c is (0~60):(100~40).

5. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that: The average particle size of the terpolymer microspheres is 500 to 1600 nm; Taking the total molar amount of the terpolymer microspheres as 100% molar amount, the molar content of the structural unit A is 49-50%; the molar content of the structural unit B is 15-45%; and the molar content of the structural unit C is 10-40%.

6. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that: Based on 100 parts by weight of the degradable copolyester, the amount of the opening agent is 0.1 to 1.5 parts by weight.

7. The easy-opening controlled biodegradable blown film material according to claim 3, characterized in that: The monomer a is terephthalic acid and / or dimethyl terephthalate.

8. The easy-opening controlled biodegradable blown film material according to claim 3, characterized in that: The monomer b is 1,3-propylene glycol and / or 1,4-butanediol.

9. The easy-opening controlled biodegradable blown film material according to claim 3, characterized in that: The monomer c is selected from at least one of succinic acid, dimethyl succinate, adipic acid or dimethyl adipate.

10. The easy-opening controlled biodegradable blown film material according to claim 3, characterized in that: The monomer d is at least one of pyromellitic dianhydride, propylene glycol or pentaerythritol.

11. The easy-opening controlled biodegradable blown film material according to claim 5, characterized in that: The average particle size of the terpolymer microspheres is 800-1600 nm.

12. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that Contains a lubricant; wherein, based on 100 parts by weight of the degradable copolyester, The amount of the lubricant is 0.05 to 5 parts; The lubricant is selected from stearates and / or organic carboxylic acid amides, wherein the stearates are selected from calcium stearate, and the organic carboxylic acid amides are selected from at least one of erucic acid amide, oleic acid amide, stearic acid stearamide, and N,N'-ethylene bis stearamide.

13. The easy-opening controlled biodegradable blown film material according to claim 12, characterized in that: Taking the amount of the degradable copolyester as 100 parts by weight, The amount of the lubricant is 0.05 to 2 parts; The organic carboxylic acid amide is selected from N,N'-ethylene bis stearamide.

14. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that Containing a nucleating agent; wherein, based on 100 parts by weight of the degradable copolyester, The weight of the nucleating agent is 0.1 to 20 parts; The nucleating agent is selected from at least one of hyperbranched polyamide, low density polyethylene, ethylene-methacrylic acid ionomer or ethylene-butyl acrylate-glycidyl methacrylate terpolymer.

15. The easy-opening controlled biodegradable blown film material according to claim 14, characterized in that: Based on 100 parts by weight of the degradable copolyester, the weight of the nucleating agent is 0.5 to 5 parts.

16. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that Contains a degradable resin; wherein, based on 100 parts by weight of the degradable copolyester, The weight of the degradable resin is 2 to 20 parts; and / or, The degradable resin is selected from at least one of polycaprolactone, butylene succinate, polyglycolic acid, polylactic acid, polyhydroxyalkanoate (PHA), and polymethyl ethylene carbonate (PPC).

17. The easy-opening controlled biodegradable blown film material according to claim 16, characterized in that: Based on 100 parts by weight of the degradable copolyester, the weight of the degradable resin is 4 to 12 parts.

18. The easy-opening controlled biodegradable blown film material according to claim 1, characterized in that Containing an antioxidant; wherein, based on 100 parts by weight of the degradable copolyester, The weight of the antioxidant is 0.05 to 5 parts; The antioxidant is a hindered phenol antioxidant and a phosphite antioxidant mixed in a mass ratio of 1:3 to 3:1; wherein the hindered phenol antioxidant is selected from at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid or 1,3,5-trimethyl-2,4,6-tris(3,5-tert-butyl-4-hydroxybenzyl)benzene; and the phosphite antioxidant is selected from at least one of tris[2.4-di-tert-butylphenyl]phosphite, distearyl pentaerythritol diphosphite or 2,2'-ethylenebis(4,6-di-tert-butylbenzene)fluorophosphite.

19. The easy-opening controlled biodegradable blown film material according to claim 18, characterized in that: Based on 100 parts by weight of the degradable copolyester, the weight of the antioxidant is 0.05 to 2 parts.

20. The method for preparing an easy-opening controlled biodegradable blown film material according to any one of claims 1 to 19, characterized in that The following steps are involved: The components including the degradable copolyester and the opening agent are mixed and then extruded and granulated to obtain the easy-opening controllable biodegradable blown film material.

21. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 20, characterized in that: In the extrusion granulation step, the processing temperature is 150-200° C. and the screw speed is 250-350 rpm.

22. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 20, characterized in that: The preparation method of the degradable copolyester comprises the following steps: The degradable copolyester is obtained by reacting components including monomer a, monomer b, monomer c and monomer d under the action of a catalyst, and then extruding the components with an organic peroxide.

23. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 22, characterized in that: The preparation method of the degradable copolyester comprises the following steps: 1) Preparation of long-chain branched aliphatic aromatic copolyester: under the action of a catalyst, monomer a, monomer b, monomer c and monomer d are mixed for esterification reaction, or the esterification product of monomer a and monomer b and the esterification product of monomer c and monomer d are mixed for co-condensation reaction to obtain long-chain branched aliphatic aromatic copolyester; 2) Extruding the long-chain branched aliphatic aromatic copolyester prepared in step 1) and an organic peroxide to obtain the degradable copolyester.

24. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 23, characterized in that: The monomer a is an aromatic dibasic acid or an ester derivative thereof; the monomer b is a C2-C 10 Aliphatic diols or C3-C 10 One or more of alicyclic diols; the monomer c is C4-C 20 The monomer d is one or more of a polyol with a functionality greater than 2, a polycarboxylic acid with a functionality greater than 2, or an anhydride with a functionality greater than 2; The amount of each monomer used is: the molar ratio of (a+c):b is 1:(0.8-3), the molar ratio of (a+c):d is 100-2000:1, and the molar ratio of a:c is (0-60):(100-40).

25. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 22, characterized in that: The catalyst contains at least one of a first catalyst, a second catalyst and a third catalyst; The first catalyst is selected from at least one of an oxide of M, M(OR1)n and M(OOCR2)m, wherein M is titanium, antimony or zinc, n and m are each independently the valence state of M, and R1 is C1-C 10 Alkyl, R2 is C1-C 20 The alkyl group; and / or, The second catalyst is a compound of RE(R3)3, wherein RE is a rare earth metal element, R3 is selected from at least one of halogen, alkoxy, aryloxy, acetylacetonato and R4COO-, and R4 is C1-C 30 The alkyl group; and / or, The third catalyst is at least one organotin compound.

26. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The first catalyst is selected from at least one of alkoxytitanium, antimony acetate, zinc acetate, zinc oxide, antimony oxide and titanium oxide.

27. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 26, characterized in that: The first catalyst is selected from at least one of tetrabutyl titanate (Ti(OC4H9)4), isopropoxy titanium, titanium dioxide, antimony trioxide, antimony acetate and zinc acetate.

28. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The RE is selected from at least one of lanthanum, cerium, praseodymium, neodymium, terbium, ytterbium, dysprosium, samarium or scandium; the halogen is chlorine or bromine, the alkoxy is a C3-C6 alkoxy, the aryloxy is an aryloxy including at least one benzene ring and / or naphthalene ring, and R4 is C1-C 20 of alkyl.

29. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 28, characterized in that: The RE is selected from lanthanum, cerium, praseodymium, neodymium or scandium, the alkyl in the alkoxy is at least one of isopropyl, n-butyl or isopentyl, the aryl in the aryloxy is at least one of 2,6-di-tert-butyl-4-methylphenyl or 4-butylphenyl, and R4 is C3-C 18 At least one of the alkyl groups.

30. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The second catalyst is at least one of lanthanum acetylacetonate, neodymium acetylacetonate, neodymium isopropoxide, lanthanum isopropoxide, scandium isopropoxide, lanthanum stearate, neodymium stearate, lanthanum chloride, tris(2,6-di-tert-butyl-4-methylphenoxy)lanthanum and hydrates thereof.

31. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The third catalyst is selected from at least one of dibutyltin oxide, methylphenyltin oxide, tetraethyltin, hexaethyltin oxide, hexacyclohexylditin oxide, didodecyltin oxide, triethylhydroxytin, triphenylhydroxytin, triisobutyltin acetate, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin sulfide, butylhydroxytin oxide, methylstannic acid, ethylstannic acid and butylstannic acid.

32. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The third catalyst is selected from a mixture of at least two of dibutyltin oxide, tetraethyltin, triphenylhydroxytin, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin sulfide, butyltin hydroxide, methylstannic acid, ethylstannic acid and butylstannic acid; when two components are selected, the total molar amount of the third catalyst is 100 mol%, and the content of each component of the third catalyst is 10 to 90 mol%.

33. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 32, characterized in that: When two components are selected, the content of each component of the third catalyst is 30-70 mol %, based on the total molar amount of the third catalyst being 100 mol %.

34. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 25, characterized in that: The molar ratio of the total amount of the catalyst to the monomer (a+c) is 1:(1000-20000); and / or, The molar ratio of the first catalyst: the second catalyst: the third catalyst is (0.1-20): (0.1-10):

1.

35. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 22, characterized in that: The amount of the organic peroxide is 0.01 to 5 wt% of the amount of the long-chain branched aliphatic aromatic copolyester; The organic peroxide is selected from organic peroxides with a half-life of 0.2 to 10 minutes within the processing temperature range.

36. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 35, characterized in that: The amount of the organic peroxide is 0.01 to 1 wt% of the amount of the long-chain branched aliphatic aromatic copolyester; The organic peroxide is selected from organic peroxides with a half-life of 0.2 to 2 minutes within the processing temperature range.

37. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 36, characterized in that: The organic peroxide is at least one selected from alkyl peroxides, acyl peroxides and peroxyesters.

38. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 37, characterized in that: The organic peroxide is selected from at least one of 2,5-bis(tert-amyl peroxy)-2,5-dimethylhexane, 2,5-bis(tert-butyl peroxy)-2,5-dimethylhexane, 3,6-bis(tert-butyl peroxy)-3,6-dimethyloctane, 2,7-bis(tert-butyl peroxy)-2,7-dimethyloctane, 8,11-bis(tert-butyl peroxy)-8,11-dimethyloctadecane or a mixture thereof, bis(alkyl peroxy)benzene, and bis(alkyl peroxy)alkyne; Wherein, the bis(alkylperoxide)benzene is selected from α,α'-(tert-amylperoxide-isopropyl)benzene, α,α'-bis(tert-butylperoxide-isopropyl)benzene or a mixture thereof; The bis(alkyl peroxy)alkyne is selected from at least one of 2,7-dimethyl-2,7-di(tert-butyl peroxy)-octanediyne-3,5,2,7-dimethyl-2,7-di(peroxyethyl carbonate)-octanediyne-3,5,3,6-dimethyl-3,6-di(peroxyethyl carbonate)octanediyne-4,3,6-dimethyl-3,6-di(tert-butyl-peroxy)octanediyne-4,2,5-dimethyl-2,5-di(peroxy-n-propyl-carbonate)hexyn-3,2,5-dimethyl-2,5-di(peroxy-isobutyl carbonate)hexyn-3,2,5-dimethyl-2,5-di(peroxyethyl monocarbonate)hexyn-3,2,5-dimethyl-2,5-di((α-cumyl peroxy)hexyn-3,2,5-dimethyl-2,5-di(tert-butyl peroxy)hexyn-3.

39. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 23, characterized in that: In step 1), The esterification reaction temperature is 150-220°C; The co-condensation reaction conditions include: temperature of 250-270°C and time of 2-3 hours; and / or, The long-chain branched aliphatic aromatic copolyester prepared in step 1) has a melt index of 5 to 100 g / 10 min at 190° C. and a load of 2.16 kg; and / or, In step 2), the extrusion temperature is 150-200°C.

40. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 39, characterized in that: In step 2), the extrusion temperature is 160-180°C.

41. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 20, characterized in that: Also includes antioxidants; The fatty aromatic copolyester is firstly mixed with an antioxidant to form granules to obtain a base resin, which is then mixed with components including an antiblocking agent and then extruded to form granules.

42. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 20, characterized in that: The preparation method of the opening agent comprises the following steps: In an inert atmosphere, components including polymerization monomers and initiators are dissolved in a reaction medium to form a homogeneous solution; the homogeneous solution is polymerized to obtain a copolymer emulsion suspension, and then centrifuged to obtain the terpolymer microspheres; Wherein, the polymerizable monomers include maleic anhydride, styrene and α-methylstyrene; Based on the total amount of the polymerized monomers, the molar content of maleic anhydride is 48 to 51%; The molar ratio of styrene to α-methylstyrene is 9:1 to 1:9; The amount of the polymerizable monomer used is 4-22 wt % of the total weight of the homogeneous solution.

43. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 42, characterized in that: Based on the total amount of the polymerized monomers, the molar content of maleic anhydride is 49 to 50%; The molar ratio of styrene to α-methylstyrene is 6:1 to 1:6; The amount of the polymerizable monomer used is 15-22 wt % of the total weight of the homogeneous solution.

44. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 42, characterized in that: The reaction medium is an organic acid alkyl ester.

45. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 44, characterized in that: The general formula of the organic acid alkyl ester is R1COOR2, wherein R1 is selected from H, C 1-4 At least one of an alkyl group, a phenyl group and a benzyl group, R2 is C 1-10 of alkyl.

46. ​​The method for preparing the easy-opening controlled biodegradable blown film material according to claim 45, characterized in that: The R1 is C 1-4 alkyl and / or phenyl, R2 is C 1-7 of alkyl.

47. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 44, characterized in that: The reaction medium is selected from at least one of ethyl formate, propyl formate, isobutyl formate, pentyl formate, ethyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, pentyl acetate, isoamyl acetate, benzyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate, isoamyl butyrate, ethyl isovalerate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate and ethyl phenylacetate.

48. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 42, characterized in that: The initiator is used in an amount of 0.4 to 4 wt % of the total weight of the homogeneous solution; The initiator is an organic peroxide and / or an azo compound; the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate; The azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

49. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 42, characterized in that: The polymerization reaction conditions include: polymerization temperature of 60 to 95° C.; polymerization time of 2 to 24 hours.

50. The method for preparing the easy-opening controlled biodegradable blown film material according to claim 49, characterized in that: The polymerization reaction conditions include: polymerization temperature of 65-76° C.; polymerization time of 4-8 hours.

51. A film made of the easy-opening controlled biodegradable blown film material according to any one of claims 1 to 19 or the material prepared by the method according to any one of claims 20 to 50, characterized in that: The thickness of the film is 5 to 100 μm; and / or, The tensile fracture stress of the film is greater than 18 MPa; and / or, The light transmittance of the film is above 89%.

52. The film according to claim 51, characterized in that: The thickness of the film is 10 to 20 μm; and / or, The tensile fracture stress of the film is greater than 25 MPa.

53. The method for preparing a thin film according to claim 51, characterized in that: The easy-opening controllable biodegradable blown film material is blown into a film to obtain the film.

54. The method for preparing a thin film according to claim 53, characterized in that: The film blowing temperature is 150-210°C; and / or, During the film blowing process, the blowing ratio is 1.5-3.

55. The method for preparing a thin film according to claim 54, characterized in that: The film blowing temperature is 175-195°C; and / or, During the film blowing process, the blowing ratio is 2 to 2.

5.

56. Use of the film according to any one of claims 51 to 54 in agricultural mulch films and packaging bag films.

Citation Information

Patent Citations

  • High-strength ultrathin biodegradable film and preparation method thereof

    CN112521727A

  • Terpolymer microspheres as well as preparation method and application thereof

    CN112708018A

  • Sealing composition and method of use thereof

    CA795843A

  • Multipolymer micro-nano particles and preparation method thereof

    CN107417840A

  • Biodegradable blended film and preparation method thereof

    CN109486083A