A method for separating and extracting valuable metals from aluminum-containing waste batteries
By adopting a manganese-containing high-aluminum slag system and oxygen and sulfur potential control in the pyrometallurgical process, the problems of high-temperature smelting and pre-aluminum removal in the pyrometallurgical process are solved, and efficient valuable metal separation and manganese resource recovery are achieved. , reducing energy consumption and process complexity, and converting cobalt, nickel, and copper into easy-to-handle metal sulfides.
Patent Information
- Application Number
- CN202111628223.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Existing pyrometallurgical processes require high-temperature smelting or pre-aluminum removal when processing scrap lithium-ion batteries containing aluminum, which increases process complexity and energy consumption. At the same time, the produced iron-cobalt-copper alloy is difficult to further separate and utilize.
The manganese-containing high-aluminum slag system is used for smelting. By controlling the oxygen potential and sulfur potential, stable sulfides are formed to separate valuable metals, reduce the amount of slagging agent, and directly enrich manganese in the slag to improve process efficiency.
Significantly reduces the amount of slag-making agent used in the smelting of high-aluminum materials, improves the economic benefits of the process, and the obtained slag can be used as raw material for subsequent manganese extraction, solving the problem of manganese resource recovery, and converting cobalt, nickel, and copper into easy-to-process metal sulfide It solves the problems of high alloy hardness and poor corrosion resistance.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recovery and environmental protection, and in particular relates to a method for separating and extracting valuable metals in waste batteries containing aluminum. Background Art
[0002] In recent years, the lithium-ion battery electric vehicle industry has been growing rapidly. Based on the battery life of 3-5 years, a large number of waste lithium-ion batteries will be generated in the future. Lithium-ion batteries are rich in valuable metals such as cobalt, nickel, and copper, and the total content of copper, cobalt, and nickel exceeds 10wt%. In addition, a large number of waste lithium-ion batteries will cause serious environmental problems if they are not properly disposed of. For this reason, the development of waste lithium-ion battery recycling and treatment technology has attracted widespread attention.
[0003] At present, the recycling and processing technologies of valuable metals in waste lithium-ion batteries are mainly divided into two categories: hydrometallurgy and pyrometallurgy. The hydrometallurgical process mainly consists of disassembly and crushing, physical sorting, acid leaching, extraction and separation. It has the advantages of low investment and construction costs, simple operation and easy implementation. However, it can generally only be used for the treatment of specific types of materials, and it is difficult to adapt to the recycling of other types or batteries with different compositions. The pyrometallurgical process is to put the battery materials into a high-temperature smelting furnace, focusing on regulating the composition of the smelting slag, allowing the impurity elements to enter the slag, and then separate them from the valuable components (copper / cobalt / nickel) alloy. Typical processes can be found in U.S. patent document with publication number US2005 / 0235775A1 and Chinese patent documents CN103526035A, CN103924088A, CN103370427A, CN103459623A, CN103380218A, CN111996377A and CN103459624A.
[0004] The biggest feature of the pyrometallurgical process is its strong adaptability to complex materials, large processing capacity, stable slag structure and low risk of secondary pollution. Therefore, it is very suitable for the disposal and resource recovery of large-scale scrapping of waste lithium-ion batteries in the future. However, unlike traditional ores, waste lithium-ion batteries and their waste materials generally contain a large amount of metallic aluminum. During the pyrometallurgical smelting process, metallic aluminum will be oxidized and enter the slag in the form of aluminum oxide. In order to maximize the capacity of aluminum oxide and improve the fluidity of the slag, a high-temperature smelting process must be adopted for smelting using a conventional slag system, and the smelting temperature must reach above 1600°C; or aluminum must be removed in advance to prevent excessive aluminum from entering the slag, thereby deteriorating the various properties of the slag. For example, Chinese patent application CN111996377A discloses a method for recovering nickel, cobalt and manganese metals from lithium-extracted materials containing aluminum waste batteries, which uses lithium-extracted materials with aluminum removed in advance as raw materials for pyrometallurgy, but this increases the complexity of the process. At the same time, wet aluminum removal, the moisture content of the residue after lithium extraction is high, and it cannot be directly smelted by high-temperature pyrometallurgy. A large amount of water must be removed in advance, thereby increasing energy consumption. In addition, existing pyrometallurgical processes mostly recover valuable metals in the form of nickel-cobalt-copper multi-element alloys. However, since their main phase compositions, iron-cobalt alloys, copper alloys, and silicon-solution iron-cobalt-copper alloys are all corrosion-resistant alloy phases, they are not only hard and difficult to break, but also have poor acid leaching properties, making subsequent wet smelting treatment difficult and not conducive to subsequent metal separation and purification. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the shortcomings and defects mentioned in the above background technology and provide a method for separating and extracting valuable metals in aluminum-containing waste batteries. The method adopts a manganese-containing high-aluminum slag system, which can significantly reduce the amount of slag-making agent used in smelting high-aluminum materials, and directly produce nickel / cobalt sulfide products that are easy to subsequently process, with good comprehensive economic benefits and high safety.
[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0007] A method for separating and extracting valuable metals from aluminum-containing waste batteries comprises the following steps: adding the aluminum-containing waste batteries, a slag-forming agent and a sulfur-containing material into a smelting furnace for smelting, so that the smelting produces matte containing Co and / or Ni, Mn-containing slag and smoke; the Mn-containing slag produced by the smelting contains MnO, CaO, SiO2, Al2O3, and may contain at least one of FeO and MgO, wherein the mass percentage of Mn is ≥5%, the total mass percentage of Mn and Fe is 5% to 40%, the mass percentage of Al2O3 is 20% to 35%, and the ratio of the total mass of CaO and MgO to the mass of SiO2 is (CaO+MgO) / SiO2≥0.3.
[0008] During the smelting process, almost all of the metallic aluminum in the waste battery is oxidized, and then enters the slag phase in the form of Al2O3. Generally speaking, the increase in the Al2O3 content in the slag will deteriorate the various properties of the slag, such as increasing the viscosity and melting temperature of the slag, which is not conducive to slag / gold separation. Based on our latest research results, by controlling the appropriate oxygen potential and sulfur potential, the manganese-containing high-aluminum slag system of the present invention can be obtained. The slag type has the advantages of high Al2O3 solubility and low solubility of valuable metals (Co, Ni). When the slag type is used to treat high-aluminum waste lithium-ion batteries and their materials, there is no need to remove aluminum in advance, which can effectively reduce the amount of slag-making agent, ensure that more aluminum oxide is contained in the slag, and improve the process efficiency. In addition, the present invention directly enriches the manganese in the waste lithium-ion batteries and their materials in the slag. Since the slag has a higher solubility for Al2O3, the corresponding amount of slag produced is less, and the grade of manganese in the slag is also higher than that in the traditional process. The obtained slag can be used as a raw material for subsequent manganese extraction.
[0009] The technical scheme of the present invention is to add aluminum-containing waste batteries, slag-forming agents and sulfur-containing materials into a smelting furnace for smelting. By controlling the appropriate oxygen potential and sulfur potential, Cu, Co and Ni can form stable sulfides and enter the matte phase, while Fe, Mn, Ca, Al, Si and other elements easily form oxides and enter the slag phase, thereby realizing the separation of valuable metals Co, Ni and Cu from other impurity elements. In industry, the oxygen potential and sulfur potential in the furnace are difficult to measure directly, but can be indirectly characterized. Under the appropriate oxygen potential and sulfur potential, at least 80% of Co and / or Ni in various materials entering the furnace enter the matte phase, and at least 40% of Mn enters the slag phase. The control of the oxygen potential and sulfur potential in the furnace is mainly achieved by adjusting the addition ratio of the reducing agent (mainly the externally added reducing carbon-containing materials and the metal aluminum, graphite, etc. in the battery), the oxidizing agent (mainly the externally added oxidizing materials and the metal oxides, etc. in the battery) and the sulfur-containing material in the furnace materials. Preferably, the mass of the slag-forming agent is controlled to be more than 0.3 times the mass of the aluminum-containing waste battery, and the mass of the sulfur-containing material is controlled to be more than 0.02 times the mass of the aluminum-containing waste battery. More preferably, the mass of the slag-forming agent is 0.3-1.5 times the mass of the aluminum-containing waste battery, and the mass of the sulfur-containing material is 0.05-2.0 times the mass of the aluminum-containing waste battery.
[0010] In the above method, preferably, the slag-making agent includes Ca-containing materials and Si-containing materials, the Ca-containing materials are one or more of limestone, dolomite, and fluorite, and the Si-containing materials are one or more of river sand, silica, and clay.
[0011] In the above method, the added sulfur-containing material can provide a sulfur source for smelting metal sulfides containing cobalt, nickel and copper. Preferably, the sulfur-containing material is one or more of elemental sulfur, copper sulfide ore, nickel sulfide ore, cobalt sulfide ore, manganese sulfide ore, pyrite, matte, and nickel matte (nickel matte). More preferably, in order to obtain a higher-grade manganese-containing slag to facilitate the subsequent recovery of manganese resources, the sulfur-containing material is manganese sulfide ore.
[0012] The reducing substances and oxidizing substances other than aluminum-containing waste batteries are collectively referred to as oxygen potential regulators. In order to adjust the oxygen potential and sulfur potential to a suitable range, preferably, the material added to the smelting furnace also includes an oxygen potential regulator, and the oxygen potential regulator is one or more of coke, coal, heavy oil, petroleum coke, natural gas, oxygen, air, pyrolusite, manganese carbonate, ferromanganese alloy, laterite nickel ore, copper oxide ore, and hydrocobaltite. More preferably, in order to avoid adding additional gangue components, the oxygen potential regulator is at least one of coke, coal, heavy oil, petroleum coke, natural gas, oxygen, and air; in order to further improve the manganese grade in the slag, the oxygen potential regulator is at least one of pyrolusite, manganese carbonate, and ferromanganese alloy.
[0013] In the above method, preferably, the mass of the oxygen potential regulator is 0-5 times the mass of the aluminum-containing waste battery.
[0014] In the above method, preferably, the smelting temperature is 1300°C-1600°C, and the smelting time is ≥20min. Coordinating the smelting parameters within the scope of the present invention is beneficial to the regulation of oxygen potential and sulfur potential during the smelting process.
[0015] The above method directly converts cobalt, nickel and copper in aluminum-containing waste batteries into metal sulfides containing cobalt, nickel, copper and the like that are easy to crush and process, which not only solves the problem that the iron-cobalt-nickel-copper alloy produced by the existing process is difficult to be further separated and utilized, but can also be directly used for the production of nickel sulfate and cobalt sulfate products for battery production. Preferably, the mass percentage of S in the matte containing Co and / or Ni is 10%-40%.
[0016] In the above method, preferably, the aluminum-containing waste battery is one or more of waste lithium-ion batteries, manganese-containing dry batteries, and waste nickel-hydrogen batteries. More preferably, the aluminum-containing waste battery is a waste lithium-ion battery. Waste lithium-ion batteries refer to discarded or invalid lithium-ion batteries, battery packaging materials or other battery products, regardless of their mechanical or electrical integrity, and specifically can be waste lithium-ion batteries containing at least one of Cu, Co, and Ni, or waste generated in the production of lithium-ion batteries. Further preferably, the waste lithium-ion batteries are one or more of waste aluminum shell lithium-ion batteries, waste polymer lithium-ion batteries, and waste steel shell lithium-ion batteries.
[0017] In the above method, preferably, the mass percentage of Al in the aluminum-containing waste battery is ≥ 2%. More preferably, the mass percentage of Al in the aluminum-containing waste battery is ≥ 5%.
[0018] The above method takes into account that aluminum-containing waste batteries generally contain a large amount of graphite and electrolyte, and directly entering the high-temperature furnace for smelting will pose an explosion safety risk. At the same time, a large amount of reducing substances are directly introduced into the furnace, which increases the difficulty of controlling the high-temperature smelting process. Preferably, the aluminum-containing waste batteries are calcined in advance, and then the calcined aluminum-containing waste batteries, slag-forming agents, and sulfur-containing materials are added to the smelting furnace for smelting.
[0019] In the above method, preferably, the material added to the smelting furnace also includes an oxygen potential regulator, and the mass of the oxygen potential regulator is 0-1 times the mass of the aluminum-containing waste battery. Compared with the treatment method without roasting, since a part of the reducing substances in the aluminum-containing waste battery can be removed during the roasting process, the amount of the subsequent oxygen potential regulator can be reduced, thereby improving the economic benefits.
[0020] In the above method, preferably, the temperature of the roasting treatment is 200°C-800°C, and the time of the roasting treatment is ≥5 minutes. More preferably, the temperature of the roasting treatment is 200°C-600°C, and the time of the roasting treatment is 10 minutes-180 minutes. Controlling the roasting parameters within the scope of the present invention is conducive to reducing the control difficulty and safety risks in the smelting stage, and can also reduce the use of oxidants in the smelting stage.
[0021] Compared with the prior art, the advantages of the present invention are:
[0022] (1) The method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention provides a new type of smelting slag. Under appropriate composition conditions, even when the Al2O3 content in the slag is as high as 20% or more, the required smelting temperature can still be controlled below 1600°C. Therefore, it is very suitable for the smelting of waste lithium-ion batteries with high aluminum content and their materials, and can effectively reduce the amount of slag-forming agent used, thereby reducing the energy consumption of the process.
[0023] (2) The method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention directly enriches manganese in waste lithium-ion batteries and materials thereof in slag, and the obtained slag can still be used as a raw material for subsequent manganese extraction, thus solving the problem of recycling manganese resources in waste batteries.
[0024] (3) The recycling method of aluminum-containing waste batteries of the present invention pre-calcines the aluminum-containing waste batteries, which can effectively avoid the safety risks caused by directly feeding the aluminum-containing waste batteries into the furnace. It also reduces the control difficulty of the smelting stage and reduces the use of oxidants in the smelting stage.
[0025] (4) The method for separating and extracting valuable metals from waste aluminum batteries of the present invention can directly convert cobalt, nickel and copper in waste aluminum batteries into metal sulfides (i.e., mattes) containing cobalt, nickel, copper and the like. This solves the problem that the valuable metals are difficult to further separate and utilize due to the high hardness and corrosion resistance of the iron-cobalt-nickel-copper alloy produced by the existing process, and can also be directly used in the production of nickel sulfate and cobalt sulfate products for battery production, thereby achieving higher comprehensive economic benefits. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0027] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0029] Embodiment 1:
[0030] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps: adding aluminum-containing waste batteries (waste polymer shell lithium ion batteries, whose chemical composition is Cu 9wt.%, Co 5wt.%, Ni 1wt.%, Al15wt.%, Fe 1wt.%, Mn 22wt.%, C 15wt.%), slag-forming agents (limestone and silica), and sulfur-containing materials (elemental sulfur) into a smelting furnace for smelting, wherein the mass of the slag-forming agent is 0.8 times the mass of the aluminum-containing waste batteries, and the mass of the sulfur-containing materials is 0.1 times the mass of the aluminum-containing waste batteries.
[0031] During the smelting process, the smelting temperature is controlled to be 1480°C and the smelting time is 55 minutes, so that the smelting outputs matte containing Co and / or Ni, slag containing Mn and smoke. Among them, the S content in the matte phase is 22.07%, and the recovery rates of Co, Ni and Cu in the matte phase are 96.98%, 97.87% and 95.39% respectively; the recovery rate of Mn in the slag is 55.87%. The slag contains Co 0.44wt%, Ni 0.02wt%, Cu 0.50wt%, Mn 7wt%, Fe 0.5%, Al2O3 27.01wt%, CaO / SiO2=0.31. In this embodiment, the amount of slag-making agent used is only 0.8 times the mass of the waste battery, which is much lower than the consumption of slag-making agent in the prior art, and the economic benefit is significant.
[0032] Embodiment 2:
[0033] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps: adding aluminum-containing waste batteries (waste aluminum shell lithium ion batteries, whose chemical composition is Cu 8wt.%, Co 16wt.%, Ni 2wt.%, Al35wt.%, Fe 1wt.%, Mn 0wt.%, C 10wt.%), slag-forming agent (dolomite and river sand), sulfur-containing material (elemental sulfur), and oxygen potential regulator (pyrolusite) into a smelting furnace for smelting, wherein the mass of the slag-forming agent is 1.25 times the mass of the aluminum-containing waste batteries, the mass of the sulfur-containing material is 0.1 times the mass of the aluminum-containing waste batteries, and the mass of the oxygen potential regulator is 0.2 times the mass of the aluminum-containing waste batteries.
[0034] During the smelting process, the smelting temperature is controlled to be 1500°C and the smelting time is 45 minutes, so that the smelting outputs matte containing Co and / or Ni, slag containing Mn and smoke. Among them, the S content in the matte phase is 26.17%, and the recovery rates of Co, Ni and Cu in the matte are 90.65%, 95.94% and 94.43% respectively; the recovery rate of Mn in the slag is 45.32%. The slag contains Co 2.33wt%, Ni 0.71wt%, Cu 0.75wt%, Mn 25.38wt%, Fe 3.01%, Al2O3 24.25wt%, (CaO+MgO) / SiO2=1.25. In this embodiment, the amount of slag-making agent used is only 1.25 times the mass of the waste battery, which is much lower than the consumption of slag-making agent in the prior art, and the economic benefit is significant.
[0035] Embodiment 3:
[0036] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps: adding aluminum-containing waste batteries (waste steel shell lithium ion batteries, whose chemical composition is Cu 8wt.%, Co 16.5wt.%, Ni 2wt.%, Al6.5wt.%, Fe 24wt.%, Mn 0.1wt.%, C 16wt.%), slag-forming agent (dolomite and river sand), and sulfur-containing material (manganese sulfide ore) into a smelting furnace for smelting, wherein the mass of the slag-forming agent is 0.5 times the mass of the aluminum-containing waste batteries, and the mass of the sulfur-containing material is 0.2 times the mass of the aluminum-containing waste batteries.
[0037] In order to adjust the oxygen potential and sulfur potential in the furnace to the appropriate value, oxygen (oxygen potential regulator) needs to be introduced into the furnace during the smelting process. The mass of the oxygen potential regulator is 0.5 times the mass of the aluminum-containing waste battery. The smelting temperature is controlled to be 1425°C and the smelting time is 30 minutes, so that the smelting output is matte containing Co and / or Ni, slag containing Mn and smoke. Among them, the S content in the matte phase is 28.15%, and the recovery rates of Co, Ni and Cu in the matte are 96.45%, 97.77% and 95.02% respectively; the Mn slag rate is 50.23%. The slag contains Co0.15wt%, Ni 0.03wt%, Cu 0.28wt%, Mn 6.03wt%, Fe 12.76wt%, Al2O3 20.23wt%, CaO / SiO2=0.51. In this embodiment, the amount of slag-forming agent used is only 0.5 times the mass of the waste battery, which is much lower than the consumption of slag-forming agent in the prior art, and the economic benefit is significant.
[0038] Embodiment 4:
[0039] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps:
[0040] (1) putting aluminum-containing waste batteries (waste polymer shell lithium ion batteries, whose chemical composition is Cu 9wt.%, Co 5wt.%, Ni 1wt.%, Al 15wt.%, Fe 1wt.%, Mn 22wt.%, C 19wt.%) into a rotary kiln for roasting, controlling the roasting temperature to 500°C and the roasting time to 60min;
[0041] (2) adding the calcined aluminum-containing waste batteries, slag-forming agent (limestone and silica), and sulfur-containing material (elemental sulfur) into a smelting furnace for smelting, wherein the mass of the slag-forming agent is 0.8 times the mass of the aluminum-containing waste batteries, and the mass of the sulfur-containing material is 0.09 times the mass of the aluminum-containing waste batteries; during the smelting process, the smelting temperature is controlled to be 1500° C. and the smelting time is 30 min, so that the smelting output is matte containing Co and / or Ni, slag containing Mn, and smoke.
[0042] Among them, the S content in the matte phase is 20.86%, and the recovery rates of Co, Ni and Cu in the matte are 98.35%, 99.03% and 95.53% respectively; the recovery rate of Mn in the slag is 40.20%. The slag contains 0.45wt% Co, 0.02wt% Ni, 0.61wt% Cu, 8.34wt% Mn, 0.59% Fe, 28.21wt% Al2O3, and CaO / SiO2=0.36. In this embodiment, the amount of slag-forming agent used is only 0.8 times the mass of the waste battery, which is much lower than the consumption of slag-forming agent in the prior art. In addition, since the aluminum-containing waste battery is roasted, the safety risks caused by its direct entry into the furnace are avoided. At the same time, some reducing substances in the aluminum-containing waste battery are removed in advance, which reduces the control difficulty of the smelting stage, and there is no need to add oxygen regulator, with significant economic benefits.
[0043] Embodiment 5:
[0044] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps:
[0045] (1) putting aluminum-containing waste batteries (waste aluminum shell lithium ion batteries, whose chemical composition is Cu 8wt.%, Co16wt.%, Ni 2wt.%, Al 35wt.%, Fe 1wt.%, Mn 0wt.%, C 10wt.%) into a rotary kiln for roasting, controlling the roasting temperature to 300° C. and the roasting time to 120 min;
[0046] (2) adding the calcined aluminum-containing waste batteries and slag-forming agent (dolomite, river sand), sulfur-containing materials (elemental sulfur), and oxygen potential regulator (pyrolusite) into a smelting furnace for smelting, wherein the mass of the slag-forming agent is 1.0 times the mass of the aluminum-containing waste batteries, the mass of the sulfur-containing materials is 0.1 times the mass of the aluminum-containing waste batteries, and the mass of the oxygen potential regulator is 0.1 times the mass of the aluminum-containing waste batteries; during the smelting process, the smelting temperature is controlled to be 1400° C. and the smelting time is 45 min, so that the smelting outputs Co and / or Ni-containing matte, Mn-containing slag and smoke.
[0047] Among them, the S content in the matte phase is 25.67%, and the recovery rates of Co, Ni and Cu in the matte are 97.45%, 97.87% and 95.30% respectively; the recovery rate of Mn in the slag is 65.01%. The slag contains 0.46wt% Co, 0.03wt% Ni, 0.54wt% Cu, 10.10wt% Mn, 5.23% Fe, 20.25wt% Al2O3, and (CaO+MgO) / SiO2=1.20. In this embodiment, the amount of slag-forming agent used is only 1.0 times the mass of the waste battery, which is much lower than the consumption of slag-forming agent in the prior art. In addition, since the aluminum-containing waste battery is roasted, the safety risk caused by its direct entry into the furnace is avoided, and at the same time, some reducing substances in the aluminum-containing waste battery are removed in advance, which reduces the control difficulty of the smelting stage, and makes the mass of the oxygen potential regulator only 0.1 times the mass of the waste battery, with significant economic benefits.
[0048] Embodiment 6:
[0049] A method for separating and extracting valuable metals from aluminum-containing waste batteries of the present invention comprises the following steps:
[0050] (1) putting aluminum-containing waste batteries (waste steel shell lithium ion batteries, whose chemical composition is Cu 8wt.%, Co 16.5wt.%, Ni 2wt.%, Al 6.5wt.%, Fe 24wt.%, Mn 0.1wt.%, C 16wt.%) into a rotary kiln for roasting, controlling the roasting temperature to 700°C and the roasting time to 15 minutes;
[0051] (2) The calcined aluminum-containing waste batteries, slag-forming agent (limestone and river sand), and sulfur-containing materials (manganese sulfide ore) are added into a smelting furnace for smelting. The mass of the slag-forming agent is 0.5 times the mass of the aluminum-containing waste batteries, and the mass of the sulfur-containing materials is 0.2 times the mass of the aluminum-containing waste batteries. In order to adjust the oxygen potential and sulfur potential in the furnace to appropriate values, oxygen (oxygen potential adjuster) is also introduced into the furnace during the smelting process. The mass of the oxygen potential adjuster is 0.03 times the mass of the aluminum-containing waste batteries. The smelting temperature is controlled to be 1350° C. and the smelting time is 60 min, so that the smelting outputs Co and / or Ni-containing matte, Mn-containing slag and smoke.
[0052] Among them, the S content in the matte phase is 27.27%, and the recovery rates of Co, Ni and Cu in the matte are 90.24%, 92.14% and 90.03% respectively; the recovery rate of Mn in the slag is 55.87%. The slag contains 0.14wt% Co, 0.02wt% Ni, 0.24wt% Cu, 5.05wt% Mn, 10.23wt% Fe, 22.34wt% Al2O3, and CaO / SiO2=0.65. In this embodiment, the amount of slag-forming agent used is only 0.5 times the mass of the waste battery, which is much lower than the consumption of slag-forming agent in the prior art. In addition, since the aluminum-containing waste battery is roasted, the safety risk caused by its direct entry into the furnace is avoided. At the same time, some reducing substances in the aluminum-containing waste battery are removed in advance, which reduces the control difficulty of the smelting stage, and makes the mass of the oxygen potential regulator only 0.03 times the mass of the waste battery, with significant economic benefits.
Claims
1. A method for separating and extracting valuable metals from aluminum-containing waste batteries, characterized in that: The following steps Composition: adding aluminum-containing waste batteries, slag-forming agents and sulfur-containing materials into a smelting furnace for smelting, so that the smelting produces matte containing Co and / or Ni, Mn-containing slag and smoke; in the Mn-containing slag, the mass percentage of Mn is ≥5%, the total mass percentage of Mn and Fe is 5%-40%, the mass percentage of Al2O3 is 20%-35%, and the ratio of the total mass of CaO and MgO to the mass of SiO2 is (CaO+MgO) / SiO2≥0.3; The mass of the slag-forming agent is more than 0.3 times the mass of the aluminum-containing waste battery, and the mass of the sulfur-containing material is more than 0.02 times the mass of the aluminum-containing waste battery; The material added to the smelting furnace also includes an oxygen potential regulator, which is one or more of coke, coal, heavy oil, natural gas, oxygen, air, pyrolusite, manganese carbonate ore, ferromanganese alloy, laterite nickel ore, copper oxide ore, and hydrocobaltite; The mass of the oxygen potential regulator is 0-5 times the mass of the aluminum-containing waste battery; Control the oxygen potential and sulfur potential so that Cu, Co, and Ni can form stable sulfides and enter the matte phase, while Fe, Mn, Ca, Al, and Si elements easily form oxides and enter the slag phase; at least 80% of the Co and / or Ni of the various materials entering the furnace enter the matte phase, and at least 40% of the Mn enters the slag phase; The smelting temperature is 1300°C-1600°C, and the smelting time is ≥20min; In the matte containing Co and / or Ni, the mass percentage of S is 10%-40%; The mass percentage of Al in the aluminum-containing waste battery is ≥5%.
2. The method according to claim 1, characterized in that The slag-making agent includes Ca-containing materials and Si-containing materials. The Ca-containing materials are one or more of limestone, dolomite, and fluorite, and the Si-containing materials are one or more of river sand, silica, and clay.
3. The method according to claim 1, characterized in that: The sulfur-containing material is one or more of elemental sulfur, copper sulfide ore, nickel sulfide ore, cobalt sulfide ore, manganese sulfide ore, pyrite, matte, and nickel matte.
4. The method according to claim 1, characterized in that: The aluminum-containing waste batteries are one or more of waste lithium-ion batteries, manganese-containing dry batteries, and waste nickel-hydrogen batteries.
5. The method according to claim 1, characterized in that The aluminum-containing waste batteries are calcined in advance, and then the calcined aluminum-containing waste batteries, slag-forming agent and sulfur-containing materials are added into a smelting furnace for smelting.
6. The method according to claim 5, characterized in that The mass of the oxygen potential regulator is 0-1 times the mass of the aluminum-containing waste batteries.
7. The method according to claim 5, characterized in that The temperature of the calcination treatment is 200° C.-800° C., and the time of the calcination treatment is ≥5 min.
Citation Information
Patent Citations
Method for recovering valuable metal
CN103370427A
Valuable metal recovery method
CN103380218A
Method for recovering valuable metals
CN103459623A
Method for recovering valuable metals
CN103459624A
Method for recycling valuable metals from waste lithium ion batteries and / or other materials
CN103526035A