A 3D printed titanium mesh for skull repair containing growth factors and preparation method thereof
The skull repair titanium mesh containing growth factors is prepared through 3D printing technology, which solves the problems of low accuracy and insufficient biological activity of the finished titanium mesh in skull repair, and achieves more efficient skull tissue repair and healing.
Patent Information
- Application Number
- CN202210024476.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-11
AI Technical Summary
The existing finished titanium mesh used alone cannot effectively induce new bone formation in skull repair, and there are problems with low accuracy, sharp edges, and insufficient biological activity during the processing process.
3D printing technology is used to prepare titanium mesh for skull repair containing growth factors. By analyzing the skull defect site information, a titanium mesh model is designed and printed, and combined with dopamine microspheres, hydroxyapatite, type I collagen and silk fibroin to form a bio-ink , perform layer coverage and post-processing to improve the biological activity and accuracy of the titanium mesh.
It improves the surface roughness and biological activity of titanium mesh materials, promotes cell adhesion and osteogenesis, enhances the repair and healing effect of skull tissue, and reduces the risk of postoperative complications.
Smart Images

Figure CN114504407B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to a 3D printed growth factor-containing skull repair titanium mesh and a preparation method thereof. Background Art
[0002] Skull defects are a common secondary disease in clinical practice. They are mainly seen in various traumatic and postoperative conditions, such as electric shock, traffic accident, gunshot wounds, skull malignant tumor resection, congenital malformations, and post-skull flap decompression surgery. In principle, skull defects with a maximum diameter of more than 3 cm require skull reconstruction surgery. When the skull defect exceeds 3 cm, clinical symptoms may occur. Successful skull reconstruction must meet three requirements: (1) maintaining the integrity of the dura mater, that is, protecting the brain; (2) protecting the barrier between the brain and the outside world, that is, biomechanical stability; and (3) maintaining the normal dome-shaped shape of the head, that is, aesthetic requirements.
[0003] The ideal skull defect repair material meets the following characteristics: (1) easy to obtain; (2) high biocompatibility; (3) able to completely match the defect site and good ductility; (4) good biomechanical properties, brain barrier protection, and resistance to external forces; (5) potential to induce bone formation; (6) compatible with cranial imaging examinations; and (7) resistant to infection.
[0004] At present, the skull repair materials used in clinical practice mainly include autologous bone, allogeneic bone, xenogeneic bone and artificial materials.
[0005] Autologous bone repair is the gold standard for skull reconstruction. Autologous bone tissue has good bone conductivity and tissue compatibility, no immune rejection reaction, and low postoperative femoral leakage rate, but it has problems such as limited donor area, difficult shaping, increased secondary trauma, and high bone absorption rate of transplanted bone, which limits its clinical application.
[0006] Allogeneic bone is usually sterilized and does not cause common infectious diseases or immunogenicity. Allogeneic bone can be biologically combined with autologous tissue after surgery, allowing tissue vascularization and autologous tissue ingrowth and reconstruction. However, the high infection rate after surgery, the absorption rate of transplanted bone, and religious and ethical factors limit the clinical application of allogeneic bone in skull defects.
[0007] Allogeneic bone is abundant in source, but has strong immunogenicity. Freeze-dried bone, calcined bone and deproteinized bone used clinically are animal bone tissues that have been processed by freeze-drying, high-temperature calcination, irradiation and decalcification, removing cells, collagen and other organic components, retaining the natural pore structure and eliminating antigenicity. However, the tissue has low mechanical strength, is loose and fragile, has poor mechanical strength, and has reduced plasticity.
[0008] The artificial skull repair materials commonly used in clinical practice include hydroxyapatite, polymethyl methacrylate, polyetheretherketone and titanium mesh.
[0009] Hydroxyapatite has good biocompatibility, osteoconductivity and osteoinductivity. After implantation, calcium and phosphorus will be released from the surface of the material and absorbed by body tissues, inducing the growth of new bone tissue. However, hydroxyapatite is easily broken by external forces after surgery, and has a high postoperative infection rate. In addition, hydroxyapatite degrades too quickly in the body. It is usually used to repair small bone defects left by skull drilling. Large bone defects need to be fixed with titanium mesh.
[0010] Polymethyl methacrylate is lightweight, inexpensive, and highly plastic. It can be instantly shaped according to the shape of the bone defect and fixed securely. The main disadvantage of polymethyl methacrylate is that it is brittle and easily cracked under external forces. It also causes certain thermal damage to surrounding tissues during the curing process during surgery, and has a high probability of postoperative infection and exposure.
[0011] Polyetheretherketone (PEEK) is a fully aromatic semicrystalline thermoplastic polymer material with good biocompatibility, wear resistance and stable chemical properties. It can be sterilized by high-temperature steam or gamma irradiation. Polyetheretherketone has strong plasticity, and its elasticity, strength, thermal insulation, stability and other aspects are comparable to autologous skull, so there is generally no rejection reaction. It is X-ray penetrable, non-magnetic, and has no artifacts in CT or MRI images, and does not affect the patient's postoperative imaging analysis. However, the melting point of polyetheretherketone is extremely high (glass transition temperature 143°C, melting point reaches 343°C), making it extremely difficult to process. In addition, the PEEK rapid prototyping parts manufactured solely by 3D printing are loose in material, and the mechanical properties do not meet medical requirements. The high cost of PEEK personalized skull surgery limits its application in personalized skull repair surgery.
[0012] Titanium mesh has good biocompatibility and physical and chemical properties, can resist secondary trauma, has strong plasticity and is non-magnetic. After implantation, fibroblasts can grow into the micropores of the titanium mesh, making the titanium mesh and tissue integrated, and there is a tendency of calcification and ossification, which does not affect the X-ray examination of the skull and the electroencephalogram examination. It has a good feel, uniform and beautiful appearance, and is widely used in the field of clinical skull defect repair.
[0013] Most of the titanium meshes used in clinical practice are finished titanium meshes, which can maintain a stable spatial structure and mechanical properties, but need to be re-cut and reshaped according to different defect conditions, which usually needs to be repeated many times. In addition, manual shaping often has large errors, and the produced repair prosthesis has poor fit and low precision, and cannot fully achieve the matching effect. In addition, sharp edges are easily formed during the shaping process, which increases the risk of titanium mesh exposure after surgery. However, a single titanium mesh is a biologically inert material, has no biological activity, cannot quickly fuse with soft tissue, and cannot effectively promote bone tissue repair and regeneration. In addition, the thermal expansion and contraction of the titanium mesh alone and its fast thermal conductivity make the scalp, dura mater and surrounding skull sensitive to cold and heat, irritation problems, and cause related complications. Summary of the invention
[0014] The purpose of the present application is to provide a 3D printed titanium mesh containing growth factors for skull repair and a preparation method thereof, so as to solve the problem that the current use of finished titanium mesh alone cannot effectively induce new bone formation.
[0015] The embodiment of the present invention provides a method for preparing a 3D printed titanium mesh for skull repair containing growth factors, the method comprising:
[0016] Analyze the head to be repaired to obtain information on the skull defect;
[0017] Perform 3D printing according to the skull defect location information to obtain a titanium mesh skull model;
[0018] Adding the titanium mesh skull model into the dopamine solution to obtain a polydopamine microsphere-modified titanium mesh skull model;
[0019] obtaining microspheres loaded with growth factors;
[0020] obtaining a type I collagen solution;
[0021] A silk fibroin solution is obtained;
[0022] Mixing hydroxyapatite, the microspheres loaded with growth factors, the type I collagen solution and the silk fibroin solution to obtain 3D printing bio-ink;
[0023] According to the skull defect location information, the 3D printed bio-ink is printed into a coating and covered on the polydopamine microsphere-modified titanium mesh skull model to obtain a primary product;
[0024] The primary product is post-processed to obtain a 3D printed skull repair titanium mesh, wherein the post-processing includes freeze drying, cross-linking, analytical process and cobalt 60 25kGy dose irradiation sterilization.
[0025] Optionally, a polydopamine microsphere-modified titanium mesh skull model is obtained, specifically comprising:
[0026] Dissolve tris(hydroxymethyl)aminomethane powder in deionized water, adjust the pH to 7.5-10 by titration with dilute hydrochloric acid, dissolve dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, mix and stir for 30-120 minutes to form a dopamine solution;
[0027] The titanium mesh skull model was added to the dopamine solution and reacted with magnetic stirring at room temperature for 24 to 48 hours. The polydopamine microsphere-modified titanium mesh was washed repeatedly with pure water for 2 to 3 times and dried in a forced air drying oven at 37 to 52° C. for 12 to 24 hours to obtain the polydopamine microsphere-modified titanium mesh skull model.
[0028] Optionally, the step of obtaining microspheres loaded with growth factors specifically includes:
[0029] dissolving the polymer in dichloromethane to obtain a polymer solution;
[0030] Mixing the growth factor and the polymer solution to obtain a first emulsion;
[0031] Mixing the first emulsion and the first polyvinyl alcohol to obtain a second emulsion;
[0032] The second emulsion and the second polyvinyl alcohol are mixed and then evaporated to obtain microspheres loaded with growth factors.
[0033] Optionally, the polymer includes at least one of polycaprolactone, polyhydroxyaliphatic carboxylic acid, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polylactic acid-polycaprolactone copolymer, polyanhydride, polysaccharide, clusterin, glycosaminoglycan, chitosan, cellulose, acrylate polymer, homopolymer of glycolic acid, homopolymer of lactic acid and copolymer derived from poly(lactide-co-glycolide);
[0034] The growth factor comprises at least one of vascular endothelial growth factor, basic fibroblast growth factor, insulin-like growth factor, transforming growth factor-β, bone morphogenetic protein-2 and platelet-derived growth factor.
[0035] Preferably, the microspheres are poly(lactide-co-glycolide) (abbreviated as PLGA), and the growth factor is bone morphogenetic protein-2 (BMP-2).
[0036] Optionally, the thickness of the titanium mesh skull model is 0.4 mm to 10 mm, the mesh diameter of the titanium mesh skull model is 0.4 mm to 0.8 mm; the mass concentration of dopamine in the dopamine solution is 0.1 to 20 mg / mL; each 100 mL of the 3D printing bio-ink contains 0.1 g to 20 g of the microspheres, the diameter of the microspheres is 1 to 100 μm, and the microspheres include 0.1% to 10% of growth factors and 90% by mass fraction. % to 99.9% of polymer; each 100mL of the 3D printing bio-ink contains 0.5g to 1.5g of hydroxyapatite, and the hydroxyapatite is medical-grade nano-hydroxyapatite, and the particle size of the medical-grade nano-hydroxyapatite is 50nm-150nm; each 100mL of the 3D printing bio-ink contains 0.5g to 3g of type I collagen, and each 100mL of the 3D printing bio-ink contains 0.5g to 10g of silk fibroin.
[0037] Optionally, the step of obtaining the type I collagen solution specifically comprises:
[0038] dissolving type I collagen in a first solvent to obtain a type I collagen solution;
[0039] Wherein, the first solvent is an acetic acid solution, and the concentration of the acetic acid solution is 0.03 mol / L-0.07 mol / L.
[0040] The step of obtaining the silk fibroin solution specifically comprises:
[0041] dissolving the silk fibroin in a second solvent, and then dialyzing to obtain a silk fibroin solution;
[0042] Wherein, the second solvent is a lithium bromide solution or a calcium chloride ternary system solution.
[0043] Optionally, the freeze-drying includes a pre-freezing process and a freeze-drying process, the freezing temperature of the pre-freezing process is -80℃~-20℃, the pre-freezing time of the pre-freezing process is 3h~24h, the freezing temperature of the freeze-drying process is -50℃~37℃, the pressure of the freeze-drying process is 0.1Pa-50Pa, and the freezing time of the freeze-drying process is 24h-72h.
[0044] Optionally, the cross-linking process includes a glutaraldehyde steam cross-linking process and a thermal cross-linking process, wherein the glutaraldehyde steam cross-linking is performed in a closed container at a cross-linking temperature of 37°C to 52°C, the glutaraldehyde steam volume concentration of the glutaraldehyde steam cross-linking is 5% to 25%, and the glutaraldehyde steam cross-linking time is 2h to 12h; and the thermal cross-linking is performed in a vacuum drying oven at a thermal cross-linking temperature of 100 to 110°C, a pressure of 10 to 150 Pa, and a cross-linking time of 12 to 48h.
[0045] Optionally, the analysis process is to analyze in a blast drying oven at a temperature of 37 to 52° C. and a time of 2 to 4 days.
[0046] Based on the same inventive concept, an embodiment of the present invention further provides a 3D printed titanium mesh for skull repair containing growth factors, wherein the titanium mesh for skull repair is prepared by the preparation method of the 3D printed titanium mesh for skull repair containing growth factors as described above.
[0047] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0048] The preparation method of a 3D printed titanium mesh for skull repair containing growth factors provided in an embodiment of the present invention comprises: analyzing a head to be repaired to obtain information on a skull defect site; performing 3D printing according to the skull defect site information to obtain a titanium mesh skull model; adding the titanium mesh skull model to a dopamine solution to obtain a polydopamine microsphere-modified titanium mesh skull model; mixing hydroxyapatite, microspheres, a collagen solution and a silk fibroin solution to obtain a 3D printed bio-ink; printing the 3D printed bio-ink into a coating and covering the polydopamine microsphere-modified titanium mesh skull model, and performing post-processing to obtain a skull repair titanium mesh; the 3D printed skull repair titanium mesh of the present invention is combined with a 3D printed titanium mesh and a guided tissue regeneration layer containing growth factors, which can increase the surface roughness and biological activity of the titanium mesh material, promote the combination of the material and bone, promote cell adhesion, proliferation and induced osteogenesis, and accelerate skull tissue repair and healing.
[0049] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0051] Figure 1 It is a flow chart of the method provided by the embodiment of the present invention. DETAILED DESCRIPTION
[0052] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0053] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0054] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0055] The technical solution of the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:
[0056] During the invention process, the applicant discovered that the 3D printed titanium mesh technology solves the plasticity and fit problems of the repair material in skull repair, and the processing speed is fast, reducing the waiting time for patients; the porous through-structure similar to human bones can effectively overcome the stress shielding and low biological activity problems commonly found in implants, and at the same time minimize the heat dissipation in the cranial cavity and maintain a normal level of thermal conductivity. However, a single 3D printed titanium mesh is a biologically inert material, has no biological activity, cannot quickly fuse with soft tissue, and cannot effectively promote bone tissue repair and regeneration.
[0057] According to a typical embodiment of the present invention, a method for preparing a 3D printed titanium mesh for skull repair containing growth factors is provided, the method comprising:
[0058] S1. Analyze the head to be repaired to obtain information on the skull defect;
[0059] Specifically, a plain CT scan and an enhanced CT scan of the defective part of the head are first performed, and then a three-dimensional reconstruction is performed to determine the location, size, shape, etc. of the skull defect.
[0060] S2. Perform 3D printing according to the skull defect site information to obtain a titanium mesh skull model;
[0061] The scanned data is imported into the software to design the bone defect model, saved in STL format and imported into the 3D printer. The bone defect model is corrected and calibrated using the software, and shaped using digital equipment according to the data of the model to produce a titanium mesh that matches the defect site. The edge of the titanium mesh should exceed the edge of the defect by 1 cm. The chemical composition of the pure titanium restoration meets the standard of GB / T13810-2017 "Titanium and Titanium Alloy Processing Materials for Surgical Implants".
[0062] In some embodiments, the 3D printed titanium mesh is integrally formed, 3 to 4 integrated protruding blocks are arranged on the edge of the titanium mesh, and titanium nail holes are arranged at the ends of the protruding blocks. The thickness of the titanium mesh is 0.4 mm to 10 mm, and the mesh diameter is 0.4 mm to 0.8 mm.
[0063] The thickness of the titanium mesh is controlled to 0.4mm to 10mm in order to better meet the needs of clinical applications of skull repair. If the thickness is too large, it cannot effectively promote the combination of the material with soft and hard tissues and cannot effectively induce osteogenesis. If the thickness is too small, it is easy to form sharp edges, increasing the risk of postoperative exposure of the titanium mesh.
[0064] It can increase the surface roughness and biological activity of titanium mesh materials, promote the combination of materials and bones, promote cell adhesion, proliferation and induction of osteogenesis, and accelerate the repair and healing of skull tissue.
[0065] Controlling the mesh diameter to 0.4mm-0.8mm is beneficial to the adhesion of osteoblasts and the ingrowth of new bone, accelerating the repair and healing of skull tissue. A diameter that is too large may lead to soft tissue fluid leakage and related complications, while a diameter that is too small is not conducive to the ingrowth of soft and hard tissues, especially new bone.
[0066] S3. Obtaining a polydopamine microsphere-modified titanium mesh skull model, specifically comprising:
[0067] Dissolve tris(hydroxymethyl)aminomethane) powder in deionized water, adjust the pH value to 7.5-10 by titration with dilute hydrochloric acid, dissolve dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, and stir for 30-120 minutes to form a dopamine solution; the mass concentration of dopamine in the dopamine solution is 0.1-20 mg / mL; dopamine can undergo oxidative polymerization reaction in an alkaline (pH>7.5) aerobic environment to form polydopamine nanospheres, and as the pH value increases, dopamine gradually undergoes self-polymerization reaction to form polydopamine, and the color gradually changes from light brown to dark brown;
[0068] The titanium mesh skull model was added to the dopamine solution and reacted with magnetic stirring at room temperature for 24 to 48 hours. The polydopamine microsphere-modified titanium mesh was washed repeatedly with pure water for 2 to 3 times and dried in a forced air drying oven at 37 to 52° C. for 12 to 24 hours to obtain the polydopamine microsphere-modified titanium mesh skull model.
[0069] S4. Obtaining microspheres loaded with growth factors;
[0070] In some embodiments, obtaining microspheres loaded with growth factors comprises:
[0071] S4.1. dissolving the polymer in dichloromethane to obtain a polymer solution;
[0072] S4.2. mixing the growth factor and the polymer solution to obtain a first emulsion;
[0073] S4.3. The first emulsion and the first polyvinyl alcohol are mixed to obtain a second emulsion;
[0074] S4.4. The second emulsion and the second polyvinyl alcohol are mixed, and then evaporated to obtain microspheres loaded with growth factors.
[0075] Specifically, a certain amount of polymer for preparing microspheres is dissolved in dichloromethane (DCM) to prepare a polymer solution. 1 mL of the polymer solution is added to a glass container, and then a certain amount of growth factor is added. The above mixture is ultrasonicated for 30 seconds using an ultrasonic probe. The first emulsion is added to a certain volume of 1% polyvinyl alcohol, and the phases are vigorously stirred at 14000 rpm to obtain a second emulsion. The second emulsion is added to a certain volume of 0.1% polyvinyl alcohol 30000-70000 (Sigma), and stirred at 300 rpm for 1 hour with a homogenizer to evaporate dichloromethane. Finally, the microspheres are collected by filtration, washed several times with distilled water, and then freeze-dried in a freeze dryer. The dried microspheres are stored at 4°C until use.
[0076] In some embodiments, the polymer is a biocompatible and biodegradable polymer, specifically, it can be selected from at least one of polycaprolactone, polyhydroxyaliphatic carboxylic acid, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polylactic acid-polycaprolactone copolymer, polyanhydride, polysaccharide, clusterin, glycosaminoglycan, deacetylated chitosan, cellulose, acrylate polymer, homopolymer of glycolic acid or lactic acid and copolymer derived from poly (lactide-co-glycolide) (abbreviated as PLGA).
[0077] In some embodiments, the growth factor comprises at least one of vascular endothelial growth factor, basic fibroblast growth factor, insulin-like growth factor, transforming growth factor-β, bone morphogenetic protein-2, and platelet-derived growth factor.
[0078] Preferably, the microspheres are poly(lactide-co-glycolide) (abbreviated as PLGA), and the growth factor is bone morphogenetic protein-2 (BMP-2).
[0079] S5. Obtaining type I collagen solution;
[0080] In some embodiments, obtaining a type I collagen solution specifically comprises:
[0081] dissolving type I collagen in a first solvent to obtain a type I collagen solution;
[0082] Wherein, the first solvent is an acetic acid solution, and the concentration of the acetic acid solution is 0.03 mol / L-0.07 mol / L.
[0083] S6. obtaining a silk fibroin solution;
[0084] In some embodiments, obtaining a silk fibroin solution specifically comprises:
[0085] dissolving the silk fibroin in a second solvent, and then dialyzing to obtain a silk fibroin solution;
[0086] The second solvent is a lithium bromide solution or a calcium chloride ternary solution. In this embodiment, the molar ratio of calcium chloride / water / ethanol in the calcium chloride ternary solution is 1:8:2.
[0087] S7. mixing hydroxyapatite, the microspheres loaded with growth factors, the type I collagen solution and the silk fibroin solution to obtain 3D printing bio-ink;
[0088] In some embodiments, the diameter of the microspheres in the bio-ink is 1 to 100 μm, the concentration is 0.1 to 20 g / 100 mL, the microspheres include 0.1% to 10% growth factor and 90% to 99.9% biopolymer by mass fraction; the particle size of medical-grade nano-hydroxyapatite is 50 to 150 nm, the concentration of hydroxyapatite is 0.5 to 1.5 g / 100 mL; the concentration of type I collagen is 0.5 to 3 g / 100 mL, the concentration of silk fibroin is 0.5 to 10 g / 100 mL, and the remainder is water.
[0089] The role of hydroxyapatite is that hydroxyapatite is the main component of natural bone inorganic salts, has good osteoconductivity and biocompatibility, and is considered to be an ideal material for bone defect repair. In particular, nano-hydroxyapatite is similar to the inorganic components in natural bones. Introducing it into skull repair materials can make the materials have great advantages in mechanics and biology, and is conducive to the growth of new bone tissue and vascular tissue. The reason for controlling the particle size of hydroxyapatite to 50-150nm is that the material is easy to obtain, has good mechanical properties and osteoconductivity, and is more in line with the needs of clinical application of skull repair. If the particle size is too large, it is not conducive to the role of hydroxyapatite in guiding the tissue regeneration layer. Adhesion affects the 3D printing of 3D printed biological ink on the titanium mesh and the mechanical properties of the guided tissue regeneration layer. A too small concentration will cause hydroxyapatite to agglomerate easily, which affects the mechanical properties of the guided tissue regeneration layer. The reason for controlling the concentration of hydroxyapatite to 0.5-1.5 g / 100 mL is that the material is more in line with the needs of clinical application of skull repair in terms of mechanics and biology. A too small concentration will affect the bone conductivity of the guided tissue regeneration layer and be unfavorable for the growth of new bone tissue. A too large concentration will be unfavorable for the 3D printing of 3D printed biological ink on the titanium mesh, and the guided tissue regeneration layer will be brittle and difficult to meet the mechanical strength requirements.
[0090] Type I collagen is the main structural protein of vertebrates. It is the extracellular matrix secreted by osteoblasts during osteogenesis. It is a scaffold for calcium salt deposition and a promoter and template for the double layer of bone matrix. It can promote cell migration, adsorption, differentiation, and regulate cell growth. It has been approved by the US FDA as a biomaterial and has a series of collagen bone implant products. Type I collagen has the advantages of low immunogenicity and no toxic side effects of degradation products in the body, but its mechanical properties are poor and its degradation rate is fast. Silk fibroin has excellent biocompatibility, biodegradability and good mechanical properties, and is easy to sterilize and shape. It is widely used in ligament tissue repair, vascular tissue transplantation, cartilage tissue repair, skin tissue regeneration and neural tissue engineering, but its mechanical strength is far less than that of bone tissue, and the degradation rate of pure silk fibroin is too slow. Nano-hydroxyapatite has good osteoconductivity and biocompatibility, but single hydroxyapatite is brittle and has low toughness. Therefore, the composite use of hydroxyapatite, type I collagen and silk fibroin can solve the insufficient performance of a single material, realize the complementary advantages of various materials, and make the obtained skull repair membrane have good mechanical properties and controllable biodegradation time. The reason for controlling the concentration of type I collagen to 0.5-3g / 100mL is that the solution is easy to prepare and the material is more in line with the needs of clinical application of skull repair. The adverse effect of too large a concentration is that type I collagen dissolves slowly, and the pore size of the guided tissue regeneration layer material is too small, which is not conducive to the growth of soft and hard tissues and affects the repair and healing of skull tissue. The adverse effect of too small a concentration is that the mechanical strength of the guided tissue regeneration layer material is low and the degradation rate is fast, which is difficult to meet the needs of clinical application of skull repair.
[0091] Collagen and silk fibroin are both natural fibrous proteins with good biocompatibility and osteoinductive properties. They can stimulate the differentiation of chondrocytes and osteoblasts around the implant site to form new bone tissue. The silk fibroin concentration is controlled to be 0.5-10g / 100mL. The adverse effect of too high a concentration is that the silk fibroin dissolves slowly, the pore size of the guided tissue regeneration layer material is small, the mechanical properties are high, and the degradation time is slow, which is not conducive to the growth of soft and hard tissues and affects the repair and healing of skull tissue. The adverse effect of too low a concentration is that the mechanical strength of the guided tissue regeneration layer material is low and the degradation rate is fast, which is difficult to meet the needs of clinical applications of skull repair.
[0092] The growth factor bone morphogenetic protein-2 (BMP-2) is contained in poly (lactide-co-glycolide) (PLGA) microspheres. The growth factor can be released for a long time through slow diffusion and slow degradation of the microsphere carrier, promote the number of new capillaries and fibroblasts in the wound, and accelerate the repair and healing of skull tissue. The reason for controlling the concentration of the microspheres to 0.1-20g / 100mL is that the microspheres can release growth factors for a long time through degradation, and accelerate the repair and healing of skull tissue. The adverse effect of too large a concentration is that the degradation rate of the microspheres is slow, which affects the release of growth factors and the repair and healing of skull tissue. The adverse effect of too small a concentration is that the degradation rate of the microspheres is fast, the content of growth factors is small and the release rate is fast, which affects the repair and healing of skull tissue.
[0093] S8. According to the information of the skull defect site, the 3D printed biological ink is printed into a coating and covered on the titanium mesh skull model to obtain a primary product;
[0094] Specifically, the confirmed three-dimensional reconstruction model of the skull defect was modified, the printing parameters were set, and the obtained 3D printed bio-ink was 3D printed as a coating on the printed titanium mesh.
[0095] In some embodiments, the printing parameters are set as follows: material deposition speed: 10 mm / s, extrusion speed: 0.09 mm / min, printing layer thickness: 0.5 mm, platform molding temperature: -20 to 4°C, air pressure: 100 to 300 kpa, mesh diameter 0.4 mm to 0.8 mm, printing thickness: 2 to 4 mm, and device needle diameter 0.4 mm.
[0096] S9. Post-process the initial product to obtain a 3D printed skull repair titanium mesh.
[0097] Specifically, the obtained printed product was post-processed, including freeze drying, cross-linking, analytical process and cobalt 60 25kGy dose irradiation sterilization to obtain a 3D printed skull repair titanium mesh.
[0098] The freeze drying includes a pre-freezing process and a freeze drying process. In some embodiments, the freeze drying process conditions are: pre-freezing at -20 to -80°C for 3 to 24 hours, and then freezing and drying the body at a temperature of -50 to 37°C and a pressure of 0.1 to 50 Pa for 24 to 72 hours.
[0099] The reason for controlling the pre-freezing temperature to -20 to -80°C and the time to 3 to 24 hours is to meet the actual freeze dryer equipment parameters and product freeze-drying process requirements. If the pre-freezing temperature is too high, the pre-freezing time will be too long. If the pre-freezing temperature is too low, the equipment temperature parameters cannot be met and it will also affect the subsequent freeze-drying process product structure.
[0100] The reason for controlling the freeze-drying temperature to -50~37℃, the pressure to 0.1~50Pa, and the time to 24~72h is to meet the actual freeze dryer equipment parameters and product freeze-drying process requirements. If the freezing temperature is too high, the freezing time will be too long. If the freezing temperature is too low, the freezing speed will be too fast, which will affect the subsequent freeze-drying process product structure.
[0101] The cross-linking process includes a glutaraldehyde steam cross-linking process and a thermal cross-linking process. In some embodiments, the process conditions of glutaraldehyde steam cross-linking are: cross-linking for 2 to 12 hours at a temperature of 37 to 52°C and a glutaraldehyde vapor concentration of 10 to 30%; the thermal cross-linking is in a vacuum drying oven, with a thermal cross-linking temperature of 100 to 110°C, a pressure of 10 to 150 Pa, and a cross-linking time of 12 to 48 hours.
[0102] The reason for controlling the temperature of glutaraldehyde steam cross-linking to 37-52°C, the volume concentration of glutaraldehyde steam to 5%-25%, and the time to 2-12h is that the volume concentration of glutaraldehyde steam is too high to be achieved, and the volume concentration of glutaraldehyde steam is too low, the cross-linking temperature is low, and the cross-linking time is too long.
[0103] The reason for controlling the thermal cross-linking temperature at 100-110°C, the pressure at 10-150Pa, and the cross-linking time at 12-48h is that low thermal cross-linking temperature, long cross-linking time, and high thermal cross-linking temperature will affect the structural performance of the product.
[0104] In some embodiments, the desorption process is performed in a forced air drying oven at a desorption temperature of 37 to 52° C. and a desorption time of 2 to 4 days.
[0105] The reason for controlling the parsing temperature at 37-52°C and the parsing time at 2-4 days is that low parsing temperature and long parsing time will affect the product structure and performance.
[0106] The 3D printed growth factor-containing skull repair titanium mesh and its preparation method of the present application will be described in detail below in combination with embodiments, control examples and experimental data.
[0107] Example 1
[0108] A method for preparing a 3D printed titanium mesh for skull repair containing growth factors, the steps are as follows:
[0109] S1. Preparation of 3D-printed titanium mesh. First, perform CT plain scan and enhanced scan of the defect site on the head, and then perform 3D reconstruction to determine the location, size, shape, etc. of the skull defect; import the scan data into the software to design the bone defect model, save it in STL format and import it into the 3D printer, use the software to correct and calibrate the bone defect model, use digital equipment to shape it according to the data of the model, and make a titanium mesh that matches the defect site. The edge of the titanium mesh should exceed the edge of the defect by 1 cm. The chemical composition of the pure titanium restoration conforms to the standard GB / T 13810-2017 "Titanium and Titanium Alloy Processing Materials for Surgical Implants"; the 3D-printed titanium mesh is integrally formed, and 4 integrated protruding blocks are set on the edge of the titanium mesh, and titanium nail holes are set at the end of the protruding blocks. The thickness of the titanium mesh is 0.4 mm and the mesh diameter is 0.6 mm.
[0110] S2. Preparation of polydopamine microspheres modified titanium mesh. Dopamine can undergo oxidative polymerization in an alkaline (pH>7.5) aerobic environment to form polydopamine nanospheres. Preparation of dopamine solution: Dissolve 0.121g of tris(hydroxymethyl)aminomethane powder in 100mL of deionized water, adjust the pH to 8.5 by titration with dilute hydrochloric acid, dissolve 200mg of dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, and stir for 60min to form a dopamine solution. Add the previously obtained or prepared titanium mesh to the dopamine solution, stir under magnetic stirring at room temperature for 36h, then wash the polydopamine microspheres modified titanium mesh with pure water 2-3 times, and dry it in a forced air drying oven at 40°C for 24h.
[0111] S3, low temperature 3D printing guided tissue regeneration coating membrane. Microspheres loaded with growth factors, medical grade nanohydroxyapatite, silk protein solution and type I collagen solution are mixed to prepare 3D printing biological ink. Then the three-dimensional reconstruction model of the skull defect confirmed in step S1 is modified, the printing parameters are set, and the obtained biological ink is 3D printed on the titanium mesh obtained by 3D printing in step S2 to guide tissue regeneration coating membrane; the diameter of the microspheres in the biological ink is 1 to 100 μm, the concentration is 10g / 100mL, and the microspheres include 0.5% growth factor and 99.5% biopolymer by mass fraction; the average particle size of medical grade nanohydroxyapatite is 100nm, and the concentration of hydroxyapatite is 0.75g / 100mL; the concentration of type I collagen is 1g / 100mL, the concentration of silk protein is 3g / 100mL, and the balance is water.
[0112] The printing parameters are: material deposition speed: 10mm / s, extrusion speed: 0.09mm / min, printing layer thickness: 0.5mm, platform molding temperature: -10℃, air pressure: 200kpa, mesh diameter 0.4mm, printing thickness: 3mm, and device needle diameter 0.4mm.
[0113] S4, post-processing the printed product obtained in step S3, including freeze drying, cross-linking, analysis process and cobalt 60 25kGy dose irradiation sterilization, to obtain a 3D printed skull repair titanium mesh. Specifically, the freeze drying process conditions are: pre-freezing at -60°C for 12 hours, and then freezing and drying at a temperature of 10°C and a pressure of 10Pa for 48 hours; the glutaraldehyde steam cross-linking process conditions are: cross-linking at a temperature of 40°C and a glutaraldehyde steam concentration of 10% for 12 hours; the heat cross-linking process conditions are: cross-linking at 100°C and 100Pa in a vacuum drying oven for 48 hours; the analysis process conditions are: in a blast drying oven, the analysis temperature is 37°C and the analysis time is 2 days.
[0114] Example 2
[0115] A method for preparing a 3D printed titanium mesh for skull repair containing growth factors, the steps are as follows:
[0116] S1. Preparation of 3D-printed titanium mesh. First, CT plain scan and enhanced scan of the defect site of the head are performed, and then three-dimensional reconstruction is performed to determine the location, size, shape, etc. of the skull defect; the scan data is imported into the software for bone defect model design, saved in STL format and imported into the 3D printer, the bone defect model is corrected and calibrated using software, and the digital equipment is used to shape it according to the data of the model to produce a titanium mesh that matches the defect site. The edge of the titanium mesh should exceed the edge of the defect by 1 cm. The chemical composition of the pure titanium restoration conforms to the standard GB / T 13810-2017 "Titanium and Titanium Alloy Processing Materials for Surgical Implants"; the 3D-printed titanium mesh is integrally formed, and three integrated protruding blocks are set on the edge of the titanium mesh, and titanium nail holes are set at the end of the protruding blocks. The thickness of the titanium mesh is 0.8 mm and the mesh diameter is 0.6 mm.
[0117] S2. Preparation of polydopamine microspheres modified titanium mesh. Dopamine can undergo oxidative polymerization in an alkaline (pH>7.5) aerobic environment to form polydopamine nanospheres. Preparation of dopamine solution: Dissolve 0.121g of tris(hydroxymethyl)aminomethane powder in 100mL of deionized water, adjust the pH to 8.5 by titration with dilute hydrochloric acid, dissolve 250mg of dopamine hydrochloride powder in tris(hydroxymethyl)aminomethane solution, and stir for 80min to form a dopamine solution. Add the previously obtained or prepared titanium mesh to the dopamine solution, stir under magnetic stirring at room temperature for 24h, then wash the polydopamine microspheres modified titanium mesh repeatedly with pure water for 2 to 3 times, and dry in a forced air drying oven at 50°C for 12h.
[0118] S3, low temperature 3D printing guided tissue regeneration coating membrane. Microspheres loaded with growth factors, medical grade nanohydroxyapatite, silk protein solution and type I collagen solution are mixed to prepare 3D printing biological ink. Then the three-dimensional reconstruction model of the skull defect confirmed in step S1 is modified, the printing parameters are set, and the obtained biological ink is 3D printed on the titanium mesh obtained by 3D printing in step S2 to guide tissue regeneration coating membrane; the diameter of the microspheres in the biological ink is 1 to 100 μm, the concentration is 6 g / 100 mL, and the microspheres include 0.5% growth factor and 99.5% biopolymer by mass fraction; the average particle size of medical grade nanohydroxyapatite is 120 nm, and the concentration of hydroxyapatite is 0.5 g / 100 mL; the concentration of type I collagen is 1.5 g / 100 mL, the concentration of silk protein is 3 g / 100 mL, and the balance is water.
[0119] The printing parameters are: material deposition speed: 10mm / s, extrusion speed: 0.09mm / min, printing layer thickness: 0.5mm, platform molding temperature: -4℃, air pressure: 250kpa, mesh diameter 0.4mm, printing thickness: 2mm, and device needle diameter 0.4mm.
[0120] S4, post-processing the printed product obtained in step S3, including freeze drying, cross-linking, analysis process and cobalt 60 25kGy dose irradiation sterilization, to obtain a 3D printed skull repair titanium mesh. Specifically, the freeze drying process conditions are: pre-freezing at -50°C for 12 hours, then freezing and drying at 20°C and 20Pa for 48 hours; the glutaraldehyde steam cross-linking process conditions are: cross-linking at 40°C and 20% glutaraldehyde steam concentration for 6 hours; the heat cross-linking process conditions are: cross-linking at 105°C and 50Pa in a vacuum drying oven for 24 hours; the analysis process conditions are: in a blast drying oven, the analysis temperature is 50°C and the analysis time is 3d.
[0121] Example 3
[0122] A method for preparing a 3D printed titanium mesh for skull repair containing growth factors, the steps are as follows:
[0123] S1. Preparation of 3D-printed titanium mesh. First, perform CT plain scan and enhanced scan of the defect site on the head, and then perform 3D reconstruction to determine the location, size, shape, etc. of the skull defect; import the scan data into the software to design the bone defect model, save it in STL format and import it into the 3D printer, use the software to correct and calibrate the bone defect model, and use digital equipment to shape it according to the data of the model to make a titanium mesh that matches the defect site. The edge of the titanium mesh should exceed the edge of the defect by 1 cm. The chemical composition of the pure titanium restoration conforms to the standard GB / T 13810-2017 "Titanium and Titanium Alloy Processing Materials for Surgical Implants"; the 3D-printed titanium mesh is integrally formed, and 3 integrated protruding blocks are set on the edge of the titanium mesh, and titanium nail holes are set at the end of the protruding blocks. The thickness of the titanium mesh is 1 mm, and the mesh diameter is 0.6 mm.
[0124] S2. Preparation of polydopamine microspheres modified titanium mesh. Dopamine can undergo oxidative polymerization in an alkaline (pH>7.5) aerobic environment to form polydopamine nanospheres. Preparation of dopamine solution: Dissolve 0.121g of tris(hydroxymethyl)aminomethane powder in 100mL of deionized water, adjust the pH to 9.0 by titration with dilute hydrochloric acid, dissolve 300mg of dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, and stir for 90min to form a dopamine solution. Add the titanium mesh obtained in step S1 to the dopamine solution, and after magnetic stirring at room temperature for 48h, wash the polydopamine microspheres modified titanium mesh repeatedly with pure water for 2 to 3 times, and dry it in a forced air drying oven at 40°C for 24h.
[0125] S3, low-temperature 3D printing guided tissue regeneration coating membrane. Microspheres loaded with growth factors, medical-grade nanohydroxyapatite, silk protein solution and type I collagen solution are mixed to prepare 3D printing biological ink. The three-dimensional reconstruction model of the skull defect confirmed in step S1 is then modified, and the printing parameters are set. The obtained biological ink is 3D printed on the titanium mesh obtained by 3D printing in step S2 to guide tissue regeneration coating membrane; the diameter of the microspheres in the biological ink is 1 to 100 μm, the concentration is 15g / 100mL, and the microspheres include 0.6% growth factor and 99.4% biopolymer by mass fraction; the average particle size of medical-grade nanohydroxyapatite is 150nm, and the concentration of hydroxyapatite is 1g / 100mL; the concentration of type I collagen is 2g / 100mL, the concentration of silk protein is 3g / 100mL, and the balance is water.
[0126] The printing parameters are: material deposition speed: 10mm / s, extrusion speed: 0.09mm / min, printing layer thickness: 0.5mm, platform molding temperature: 0℃, air pressure: 250kpa, mesh diameter 0.4mm, printing thickness: 3mm, and device needle diameter 0.4mm.
[0127] S4. Post-process the printed product obtained in step S3, including freeze drying, cross-linking, analysis process and cobalt 60 25kGy dose irradiation sterilization, to obtain a 3D printed skull repair titanium mesh. Specifically, the freeze drying process conditions are: pre-freezing at -60°C for 24 hours, followed by freezing and drying at 5°C and 30Pa for 48 hours; the glutaraldehyde steam cross-linking process conditions are: cross-linking at 40°C and 25% glutaraldehyde steam concentration for 3 hours; the heat cross-linking process conditions are: cross-linking at 110°C and 30Pa in a vacuum drying oven for 24 hours; the analysis process conditions are: in a blast drying oven, the analysis temperature is 45°C and the analysis time is 3d.
[0128] Example 4
[0129] A method for preparing a 3D printed titanium mesh for skull repair containing growth factors, the steps are as follows:
[0130] S1. Preparation of 3D-printed titanium mesh. First, CT plain scan and enhanced scan of the defect site of the head are performed, and then three-dimensional reconstruction is performed to determine the location, size, shape, etc. of the skull defect of the head; the scan data is imported into the software for bone defect model design, saved in STL format and imported into the 3D printer, the bone defect model is corrected and calibrated using software, and the digital equipment is used to shape it according to the data of the model to produce a titanium mesh that matches the defect site. The edge of the titanium mesh should exceed the edge of the defect by 1 cm. The chemical composition of the pure titanium restoration conforms to the standard GB / T 13810-2017 "Titanium and Titanium Alloy Processing Materials for Surgical Implants"; the 3D-printed titanium mesh is integrally formed, and three integrated protruding blocks are set on the edge of the titanium mesh, and titanium nail holes are set at the end of the protruding blocks. The thickness of the titanium mesh is 0.6 mm, and the mesh diameter is 0.6 mm.
[0131] S2. Preparation of polydopamine microspheres modified titanium mesh. Dopamine can undergo oxidative polymerization in an alkaline (pH>7.5) aerobic environment to form polydopamine nanospheres. Preparation of dopamine solution: Dissolve 0.121g of tris(hydroxymethyl)aminomethane powder in 100mL of deionized water, adjust the pH to 9.5 by titration with dilute hydrochloric acid, dissolve 200mg of dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, and stir for 60min to form a dopamine solution. Add the titanium mesh obtained in step S1 to the dopamine solution, and after reacting for 36h under magnetic stirring at room temperature, wash the polydopamine microspheres modified titanium mesh repeatedly with pure water for 2 to 3 times, and dry it in a forced air drying oven at 45°C for 12h;
[0132] S3, low temperature 3D printing guided tissue regeneration coating membrane. Microspheres loaded with growth factors, medical grade nanohydroxyapatite, silk protein solution and type I collagen solution are mixed to prepare 3D printing biological ink. Then the three-dimensional reconstruction model of the skull defect confirmed in step S1 is modified, the printing parameters are set, and the obtained biological ink is 3D printed on the titanium mesh obtained by 3D printing in step S2 to guide tissue regeneration coating membrane; the diameter of the microspheres in the biological ink is 1 to 100 μm, the concentration is 20g / 100mL, and the microspheres include 1% growth factor and 90% biopolymer by mass fraction; the average particle size of medical grade nanohydroxyapatite is 120nm, and the concentration of hydroxyapatite is 1.5g / 100mL; the concentration of type I collagen is 3g / 100mL, the concentration of silk protein is 3g / 100mL, and the balance is water.
[0133] The printing parameters are: material deposition speed: 10 mm / s, extrusion speed: 0.09 mm / min, printing layer thickness: 0.5 mm, platform molding temperature: 4 ° C, air pressure: 300 kpa, mesh diameter 0.4 mm, printing thickness: 3 mm, and device needle diameter 0.4 mm.
[0134] S4, post-processing the printed product obtained in step S3, including freeze drying, cross-linking, analysis process and cobalt 60 25kGy dose irradiation sterilization, to obtain a 3D printed skull repair titanium mesh. Specifically, the freeze drying process conditions are: pre-freezing at -50°C for 24 hours, followed by freeze drying at 25°C and 15Pa for 72 hours; the glutaraldehyde steam cross-linking process conditions are: cross-linking at 40°C and 20% glutaraldehyde steam concentration for 6 hours; the heat cross-linking process conditions are: cross-linking at 110°C and 100Pa in a vacuum drying oven for 48 hours; the analysis process conditions are: in a blast drying oven, the analysis temperature is 45°C and the analysis time is 4d.
[0135] Comparative Example 1
[0136] Finished titanium mesh is purchased from the market, cut and shaped to produce a skull repair titanium mesh.
[0137] Experimental Example 1
[0138] The titanium mesh obtained in Example 1 and Comparative Example 1 was used in a New Zealand rabbit skull defect model. 40 New Zealand rabbit skull defect repair models were taken for the experiment and divided into a control group and a test group, with 20 cases in each group. The test group was Example 1, which used a 3D printed skull repair titanium mesh, and the control group was Comparative Example 1, which was a commercially available finished titanium mesh, which was cut and shaped to obtain a skull repair titanium mesh. The test period was 3-18 months, and the complications (incision infection, titanium mesh leakage, bone leakage, titanium mesh infection and skull asymmetry) after skull defect repair in New Zealand rabbits were observed. The results are shown in the following table:
[0139]
[0140] From the data in the table, it can be seen that the skull repair titanium mesh prepared by this method is used in the New Zealand rabbit skull defect model, and the complications are significantly lower than those in the control group. The reason may be that the titanium mesh is prepared by the 3D printing method, and it can be shaped according to different defect conditions. The titanium mesh produced has high precision, and no sharp edges are formed during the shaping process. It has a good fit with the defect site and can fully achieve a matching effect. In addition, the use of 3D printed titanium mesh and a guided tissue regeneration layer containing growth factors can increase the surface roughness and bioactivity of the titanium mesh material, and there is no risk of postoperative infection and exposure.
[0141] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0142] (1) The raw materials are easily available, safe and environmentally friendly, avoiding any hidden dangers to the human body during the preparation process and use of the final product;
[0143] (2) The titanium mesh is prepared by 3D printing, and can be shaped according to different defect conditions. The titanium mesh produced has high precision, no sharp edges are formed during the shaping process, and it fits well with the defect site, which can fully achieve the matching effect, without the risk of postoperative titanium mesh exposure;
[0144] (3) Polydopamine is mainly secreted by the foot gland of mussels, which contains a large amount of adhesion proteins. It is secreted into seawater, gradually solidifies, and forms foot threads, which firmly adhere to the surface of the substrate material. Polydopamine can promote cell adhesion and has good biocompatibility and biodegradability. As a simple and universal functional surface modification method, it has rapidly developed and been widely used. Polydopamine can not only be used to modify regular surfaces, but also to modify some complex three-dimensional surfaces, such as metals, cardiovascular stent surfaces and carbon nanotubes. After these three-dimensional surfaces are modified with polydopamine, due to its secondary reactivity, they can also be directly connected to biomolecules and drugs or combined with other coating technologies to prepare multifunctional composite coatings. When polydopamine is coated on the surface of the substrate material, it can achieve a thin thickness and strong bonding, and the surface of the substrate material can obtain good hydrophilicity and adhesion. Literature reports that the use of polydopamine coating can not only promote osteogenic differentiation and calcium mineralization in vitro, but also promote osteogenesis and increase bone integration in vivo experiments. Polydopamine nanospheres are used to modify the titanium mesh to improve its biocompatibility and bioactivity. Secondary coating modification on its surface is beneficial to the adhesion, proliferation and secretion of extracellular matrix of seed cells on the surface of the material, thus accelerating the rapid fusion of the repair material and soft tissue.
[0145] (4) Good bone conductivity, which is conducive to the growth of new bone tissue and vascular tissue. Hydroxyapatite is the main component of natural bone inorganic salts. It has good bone conductivity and biocompatibility and is considered to be an ideal material for bone defect repair. In particular, nano-hydroxyapatite is similar to the inorganic components in natural bone. When introduced into bone repair materials, it can make the materials have great advantages in mechanics and biology, which is conducive to the growth of new bone tissue and vascular tissue.
[0146] (5) Type I collagen is the main structural protein of vertebrates. It is the extracellular matrix secreted by osteoblasts during osteogenesis. It is a scaffold for calcium salt deposition and a promoter and template for the double layer of bone matrix. It can promote cell migration, adsorption, differentiation, and regulate cell growth. It has been approved by the US FDA as a biomaterial and has a series of collagen bone implant products. Type I collagen has the advantages of low immunogenicity and no toxic side effects of degradation products in the body, but its mechanical properties are poor and its degradation rate is fast. Silk fibroin has excellent biocompatibility, biodegradability and good mechanical properties. It is easy to sterilize and shape. It is widely used in ligament tissue repair, vascular tissue transplantation, cartilage tissue repair, skin tissue regeneration and neural tissue engineering. However, its mechanical strength is far less than that of bone tissue, and the degradation rate of pure silk fibroin is too slow. Nano-hydroxyapatite has good osteoconductivity and biocompatibility, but single hydroxyapatite is relatively brittle and has low toughness. Therefore, the composite use of hydroxyapatite and type I collagen and / or silk fibroin can solve the problem of insufficient performance of a single material, realize the complementary advantages of various materials, and make the obtained bone repair material have good mechanical properties and controllable biodegradation time, so that the skull repair material can maintain its morphological structure for a certain period of time or for a long time, and match the biomechanical properties of the original skull bone tissue at the implantation site;
[0147] (6) Good osteoinductivity, which can stimulate the differentiation of chondrocytes and osteoblasts around the implant site to form new bone tissue. Type I collagen and silk fibroin are both natural fibrous proteins with good biocompatibility and osteoinductivity, which are conducive to the adhesion, proliferation and secretion of extracellular matrix of seed cells on the surface of the material, accelerate the rapid fusion of the repair material and soft tissue, and can stimulate the differentiation of chondrocytes and osteoblasts around the implant site to form new bone tissue;
[0148] (7) Bone morphogenetic protein-2 (BMP-2) is considered to be the growth factor with the strongest osteoinductive ability and the ability to promote bone regeneration. It can induce undifferentiated mesenchymal stem cells to proliferate and differentiate into osteoblasts across species, thereby promoting bone repair. Bone morphogenetic protein-2 (BMP-2) is contained in poly (lactide-co-glycolide) (PLGA) microspheres. The growth factor can be released for a long time through slow diffusion and slow degradation of the microsphere carrier, promoting the number of new capillaries and fibroblasts on the wound surface, and accelerating the repair and healing of skull tissue;
[0149] (8) Composite polydopamine microspheres and a guided tissue regeneration layer containing growth factors on a titanium mesh can improve the thermal expansion and contraction of titanium mesh alone, improve thermal conductivity, and promote the sensitivity of the scalp, dura mater, and surrounding skull to heat and cold, irritation, and related complications.
[0150] (9) The 3D printing method can precisely control the micropore size and porosity of the bone repair material, which is conducive to the adhesion of seed cells and growth factors, as well as the exchange of nutrients and metabolites. Low-temperature rapid prototyping manufacturing technology (LDM) is a new type of rapid prototyping technology based on the principle of rapid prototyping technology combined with phase separation method. The difference from other rapid prototyping technologies is that the temperature in the molding chamber is controlled at around -30°C, the solution extruded by the nozzle quickly condenses at low temperature, the nozzle moves according to the program under computer control, and the printed layers are finally formed into a three-dimensional porous structure by stacking layer by layer. The properties and structure of the materials are not damaged during the material processing process, which belongs to the scope of green manufacturing.
[0151] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0152] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0153] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a 3D printed titanium mesh containing growth factors for skull repair. It is characterized in that The method comprises: Analyze the head to be repaired to obtain information on the skull defect; Perform 3D printing according to the skull defect location information to obtain a titanium mesh skull model; Adding the titanium mesh skull model into the dopamine solution to obtain a polydopamine microsphere-modified titanium mesh skull model; obtaining microspheres loaded with growth factors; obtaining a type I collagen solution; A silk fibroin solution is obtained; Mixing hydroxyapatite, the microspheres loaded with growth factors, the type I collagen solution and the silk fibroin solution to obtain 3D printing bio-ink; According to the skull defect location information, the 3D printed bio-ink is printed into a coating and covered on the polydopamine microsphere-modified titanium mesh skull model to obtain a primary product; The primary product is post-processed to obtain a 3D printed skull repair titanium mesh, wherein the post-processing includes freeze drying, cross-linking, analytical process and cobalt 60 25 kGy dose irradiation sterilization; The method of obtaining the polydopamine microsphere-modified titanium mesh skull model specifically comprises: Dissolve tris(hydroxymethyl)aminomethane powder in deionized water, adjust the pH to 7.5-10 by titration with dilute hydrochloric acid, dissolve dopamine hydrochloride powder in the tris(hydroxymethyl)aminomethane solution, and stir for 30-120 minutes to form a dopamine solution; The titanium mesh skull model is added to the dopamine solution, and reacted under magnetic stirring at room temperature for 24 to 48 hours, and then the polydopamine microsphere-modified titanium mesh is repeatedly washed with pure water for 2 to 3 times, and dried in a blast drying oven at 37 to 52° C. for 12 to 24 hours to obtain a polydopamine microsphere-modified titanium mesh skull model; The method of obtaining the microspheres loaded with growth factors specifically comprises: dissolving the polymer in dichloromethane to obtain a polymer solution; Mixing the growth factor and the polymer solution to obtain a first emulsion; Mixing the first emulsion and the first polyvinyl alcohol to obtain a second emulsion; The second emulsion and the second polyvinyl alcohol are mixed, and then evaporated to obtain microspheres loaded with growth factors; The thickness of the titanium mesh skull model is 0.4 mm to 10 mm, and the mesh diameter of the titanium mesh skull model is 0.4 mm to 0.8 mm; The mass concentration of dopamine in the dopamine solution is 0.1-20 mg / mL; the microspheres are contained in 100 mL of the 3D printing bio-ink at 0.1 g-20 g, the diameter of the microspheres is 1-100 μm, and the microspheres include 0.1%-10% growth factors and 90%-99.9% polymers by mass fraction; the 3D printing bio-ink contains 0.5 g-1.5 g hydroxyapatite per 100 mL, the hydroxyapatite is medical-grade nano-hydroxyapatite, and the particle size of the medical-grade nano-hydroxyapatite is 50 nm-150 nm; the 3D printing bio-ink contains 0.5 g-3 g type I collagen per 100 mL, and the 3D printing bio-ink contains 0.5 g-10 g silk fibroin per 100 mL; The freeze drying process includes a pre-freezing process and a freeze drying process, the freezing temperature of the pre-freezing process is -80°C to -20°C, the pre-freezing time of the pre-freezing process is 3h to 24h, the freezing temperature of the freeze drying process is -50°C to 37°C, the pressure of the freeze drying process is 0.1Pa-50Pa, and the freezing time of the freeze drying process is 24h-72h; The crosslinking includes a glutaraldehyde steam crosslinking process and a thermal crosslinking process. The glutaraldehyde steam crosslinking is carried out in a closed container at a crosslinking temperature of 37°C to 52°C, a glutaraldehyde steam volume concentration of 5% to 25%, and a glutaraldehyde steam crosslinking time of 2h to 12h. The thermal crosslinking is carried out in a vacuum drying oven at a thermal crosslinking temperature of 100 to 110°C, a pressure of 10 to 150 Pa, and a crosslinking time of 12 to 48h. The decomposition process is to decompose the sample in a blast drying oven at a temperature of 37 to 52° C. and for a time of 2 to 4 days.
2. The method for preparing the 3D printed titanium mesh for skull repair containing growth factors according to claim 1, It is characterized in that The polymer includes at least one of polycaprolactone, polyhydroxyaliphatic carboxylic acid, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polylactic acid-polycaprolactone copolymer, polyanhydride, clusterin, glycosaminoglycan, chitosan, cellulose, acrylate polymer, homopolymer of glycolic acid, homopolymer of lactic acid, and copolymer derived from poly(lactide-co-glycolide); The growth factor comprises at least one of vascular endothelial growth factor, basic fibroblast growth factor, insulin-like growth factor, transforming growth factor-β, bone morphogenetic protein-2 and platelet-derived growth factor.
3. The method for preparing the 3D printed titanium mesh for skull repair containing growth factors according to claim 1, It is characterized in that The method of obtaining the type I collagen solution specifically comprises: dissolving type I collagen in a first solvent to obtain a type I collagen solution; Wherein, the first solvent is an acetic acid solution, and the concentration of the acetic acid solution is 0.03mol / L-0.07mol / L; The step of obtaining the silk fibroin solution specifically comprises: dissolving the silk fibroin in a second solvent, and then dialyzing to obtain a silk fibroin solution; Wherein, the second solvent is a lithium bromide solution or a calcium chloride ternary system solution.
4. A 3D printed titanium mesh containing growth factors for skull repair, It is characterized in that The skull repair titanium mesh is prepared by the preparation method of 3D printing skull repair titanium mesh containing growth factors as described in any one of claims 1 to 3.