Positive electrode active material recycling method
Through the heat treatment, washing and annealing of lithium secondary battery cathode waste, the environmental protection and cost issues of cathode waste reuse in lithium secondary battery manufacturing are solved, and the efficient reuse and environmentally friendly production of cathode active materials of lithium secondary batteries are achieved.
Patent Information
- Application Number
- CN202080067379.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-06
AI Technical Summary
Existing technology cannot effectively reuse cathode waste in the manufacturing process of lithium secondary batteries, and the method of extracting active materials has environmental issues and high costs.
By thermally treating the lithium cobalt oxide cathode waste, washing and annealing the alkaline lithium compound solution in the aqueous solution, the active materials are separated and collected, avoiding acid extraction and neutralization processes, achieving environmental protection and cost reduction.
The reuse of positive active materials of lithium secondary batteries is realized, which reduces process costs, reduces environmental pollution, and improves the reusability of materials.
Smart Images

Figure CN114514647B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for recycling resources in the manufacturing process of lithium secondary batteries. More specifically, the present invention relates to a method for collecting and recycling positive electrode waste generated in the manufacturing process of lithium secondary batteries or positive electrode active materials of lithium secondary batteries discarded after use. Background Art
[0002] Rechargeable lithium secondary batteries are gaining attention as a substitute for fossil energy. They are mainly used in traditional handheld devices such as mobile phones, cameras, and power tools. Recently, the scope of application tends to be gradually expanded to vehicles driven by electricity (EV, HEV, PHEV), large-capacity energy storage systems (ESS), and uninterruptible power supply systems (UPS).
[0003] A lithium secondary battery includes: an electrode assembly including a unit cell, each unit cell including a positive plate and a negative plate, the positive plate and the negative plate including a current collector and an active material coated on the current collector, a separator interposed between the positive plate and the negative plate; and a package or battery case, in which the electrode assembly is airtightly received together with an electrolyte solution. Lithium secondary batteries mainly include lithium-based oxides as positive electrode active materials and carbon-based materials as negative electrode active materials. Lithium-based oxides contain metals such as cobalt, nickel or manganese. In particular, cobalt, nickel and manganese are very expensive precious metals. Among them, cobalt is a strategic metal, and its supply is the focus of worldwide attention. Due to the limited number of cobalt producing countries, the global supply of cobalt is unstable. When the supply and demand of strategic metals are unbalanced, the cost of raw materials is likely to rise.
[0004] There have been studies on collecting and recovering valuable metals from discarded lithium secondary batteries (waste batteries) after expiration. In addition to waste batteries, it is more preferable to collect resources from waste materials discarded after positive plate stamping, or from positive electrodes that have defects or failures during the process.
[0005] Currently, if Figure 1 As shown in , a lithium secondary battery is manufactured by coating a positive electrode slurry including a positive electrode active material, a conductive material, a binder and a solvent on a long sheet type positive electrode current collector 10 (such as aluminum (Al) foil) to form a positive electrode active material layer 20, thereby manufacturing a positive electrode sheet 30, and punching a positive electrode plate 40 into a predetermined size. The remaining portion after punching is discarded as a positive electrode waste 50. If the positive electrode active material is collected and reused from the positive electrode waste 50, it will be very ideal in terms of industrial economy and environment.
[0006] Most of the existing methods for collecting positive electrode active materials include dissolving the positive electrode with hydrochloric acid, sulfuric acid, nitric acid, etc., extracting active material elements such as cobalt, nickel, and manganese, and using them as raw materials for the synthesis of positive electrode active materials. However, the use of acid to extract active material elements uses a non-environmentally friendly process to collect pure raw materials, and requires a neutralization process and a wastewater treatment process, resulting in increased process costs. In addition, it is impossible to collect lithium, which is one of the key positive electrode active material elements. In order to overcome these shortcomings, a direct recycling method that does not dissolve the positive electrode active material and does not extract the active material in elemental form is needed. Summary of the invention
[0007] Technical issues
[0008] The present disclosure is directed to providing a method for collecting and reusing active materials from cathode waste.
[0009] Technical Solution
[0010] In order to solve the above problems, a method for recycling positive electrode active materials disclosed in the present invention comprises: (a) heat treating positive electrode waste including a lithium cobalt oxide positive electrode active material layer located on a current collector in air to thermally decompose a binder and a conductive material in the active material layer so as to separate the current collector from the active material layer, and collect the active material in the active material layer; (b) washing the collected active material with a lithium compound solution that is alkaline in an aqueous solution and drying it; and (c) annealing the washed active material with the addition of a lithium precursor to obtain a reusable active material.
[0011] The heat treatment may be performed at 300°C to 650°C.
[0012] The heat treatment may be performed at 550° C. for 30 minutes with a temperature rise rate of 5° C. / minute.
[0013] The washing may be performed by stirring the collected active material while immersing in the lithium compound solution.
[0014] The content of the lithium compound (preferably LiOH) in the lithium compound solution is greater than 0% and less than 15%. The washing may be performed within 1 hour.
[0015] The lithium precursor may be at least one of LiOH, Li2CO3, LiNO3 or Li2O.
[0016] Lithium may be added in an amount that adds a lithium precursor in accordance with a ratio of lost lithium to a ratio between lithium and other metals in an original active material used in the active material layer.
[0017] The lithium may be added in an amount of 0.001 to 0.4 in molar ratio to the lithium precursor.
[0018] The annealing may be performed in air at 400° C. to 1000° C.
[0019] The temperature of the annealing step may exceed the melting point of the lithium precursor.
[0020] The active material in the active material layer may be collected in a powder form, and carbon generated by carbonization of the binder or the conductive material does not remain on the surface.
[0021] The reusable active material may have a similar particle size distribution as the active material in the active material layer.
[0022] Another method for recycling positive active materials according to the present disclosure includes: (a) heat treating positive electrode waste in air at 300° C. to 650° C., wherein the positive electrode waste is left after punching a positive electrode plate in a positive electrode including a lithium cobalt oxide positive electrode active material layer on a current collector, and the heat treatment is used to thermally decompose the binder and the conductive material in the active material layer to separate the current collector from the active material layer, and collect the active material in the active material layer; (b) washing the collected active material with a lithium compound solution and drying it, wherein the lithium compound solution is alkaline in aqueous solution and the content of the lithium compound is above 0% and below 15%; and (c) annealing the washed active material in air at 400° C. to 1000° C. with the addition of at least one of LiOH, Li2CO3, LiNO3 and Li2O.
[0023] Beneficial effects
[0024] According to the present disclosure, it is possible to reuse discarded positive electrode active materials (such as positive electrode waste generated during the manufacture of lithium secondary batteries) without using acid, thereby achieving environmental protection. The method according to the present disclosure does not require a neutralization process or a wastewater treatment process, thereby achieving environmental mitigation and reducing process costs.
[0025] According to the present disclosure, all metal elements of the positive electrode active material can be collected. Since the current collector is not dissolved, the current collector can be collected. The extracted active material elements are not used as raw materials for synthesizing the positive electrode active material, and the active material collected in the form of powder is directly reused, thereby achieving economic benefits.
[0026] According to the present disclosure, safety is achieved because toxic and explosive solvents such as NMP, DMC, acetone, and methanol are not used, and simple processes such as heat treatment, washing, and annealing are used, so it is easy to manage and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings illustrate embodiments of the present disclosure and, together with the following detailed description, help to further understand the technical aspects of the present disclosure. Therefore, the present disclosure should not be interpreted as being limited to the accompanying drawings.
[0028] Figure 1 : is a figure which shows the positive electrode waste material discarded after punching out the positive electrode plate in the positive electrode sheet.
[0029] Figure 2 is a flow chart of an active material recycling method according to the present disclosure.
[0030] Figure 3 The results of battery evaluation using the active materials of Examples and Comparative Examples are shown.
[0031] Figure 4 X-ray diffraction (XRD) patterns of active materials of Examples and Comparative Examples are shown.
[0032] Figure 5 are scanning electron microscope (SEM) photographic images of the active materials of Examples and Comparative Examples.
[0033] Figure 6 is a graph showing the particle size distribution of the active materials of Examples and Comparative Examples. DETAILED DESCRIPTION
[0034] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms or words used in the specification and the appended claims should not be interpreted as being limited to the general and dictionary meanings, but are interpreted according to the meanings and concepts corresponding to the technical aspects of the present disclosure based on the principle of allowing the inventor to appropriately define the terms to obtain the best interpretation. Therefore, the embodiments described herein and the figures in the drawings are only examples and do not fully describe the technical aspects of the present disclosure, so it should be understood that various other equivalents and modifications may be made to them when filing a patent application.
[0035] In the following description, reference is made to the accompanying drawings which form a part of the present disclosure. The embodiments described in the detailed description, drawings, and appended claims are not intended to be limiting. Other embodiments may be used, and modifications and changes may be made thereto, without departing from the technical aspects and scope of the subject matter disclosed herein. As generally described herein and illustrated in the accompanying drawings, aspects of the present disclosure may include arrangements, substitutions, combinations, and designs of various different elements, and it will be immediately understood that all such elements are expressly contemplated.
[0036] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs (hereinafter referred to as "person skilled in the art").
[0037] The present disclosure is not limited to the specific embodiments described herein. It is obvious to those skilled in the art that many variations and changes may be made to the present disclosure without departing from the technical aspects and scope of the present disclosure. It is obvious to those skilled in the art that functionally equivalent methods within the scope of the present disclosure are apparent from the foregoing description, in addition to those methods listed herein. Such variations and changes fall within the scope of the appended claims. The scope of all equivalents to which the present disclosure and the appended claims are entitled will be defined by the appended claims. It should be understood that the present disclosure is not limited to specific variant methods. It should be further understood that the terms used herein are intended to describe specific embodiments, rather than to limit the present disclosure.
[0038] The traditional active material recycling process is mainly to extract the precious metal (nickel, cobalt, manganese) elements in the lithium secondary battery active materials whose performance has deteriorated after use, and to resynthesize the active materials. Compared with the traditional process, the feature of the present invention is to collect active materials from the positive electrode waste generated in the lithium secondary battery manufacturing process.
[0039] In addition, well-known active material recycling processes involve producing metals (direct reduction method) or resynthesizing active materials from precious metals extracted by acid / base dissolution or melted using reducing agents / additives, which requires additional chemical methods, complicates the process, and causes additional economic expenditure. However, the present disclosure relates to a method for directly recycling positive electrode active materials without dissolving the positive electrode active materials.
[0040] In order to directly reuse the positive electrode active material, it is necessary to remove the current collector from the positive electrode. The current collector can be removed from the positive electrode by removing the binder through high temperature heat treatment, melting the binder using a solvent, melting the current collector, and screening the active material through dry grinding and sieving.
[0041] When a solvent is used to melt the binder, the stability of the solvent is important. NMP is the most effective solvent, but its disadvantages are toxicity and high cost. Another disadvantage is that a waste solvent reprocessing or solvent collection process must be performed. The process cost required to melt the current collector is lower than that of using a solvent. However, it is difficult to remove impurities from the surface of the reusable active material, and hydrogen is produced during the current collector removal process, posing an explosion risk. Dry grinding and screening cannot perfectly separate the current collector and active material. The particle size distribution of the active material changes during the grinding process, and it is difficult to remove the binder, resulting in degradation of the characteristics of the battery including the reusable active material.
[0042] The present disclosure uses high temperature heat treatment to separate the active material from the current collector. In particular, the heat treatment is carried out in air, so the process only requires heating without any special device configuration, and is therefore relatively simple and suitable for large-scale production and commercialization. However, impurities should not remain on the surface of the reusable active material. The present disclosure proposes removing impurities from the surface of the reusable active material.
[0043] In the following, reference will be made to Figure 2 An active material recycling method according to one embodiment of the present disclosure is described. Figure 2 is a flow chart of an active material recycling method according to the present disclosure.
[0044] refer to Figure 2 First, discarded positive electrode scrap is prepared (S10).
[0045] As mentioned above Figure 1 As described above, the positive electrode waste can be what is left after manufacturing the positive electrode sheet including the positive electrode active material layer on the current collector and stamping the positive electrode sheet. In addition, the positive electrode waste can be prepared by collecting the positive electrode with process defects or failures. In addition, the positive electrode waste can be prepared by separating the positive electrode from the lithium secondary battery discarded after use.
[0046] For example, the positive electrode waste may be what is left after the following process: coating a slurry prepared by mixing lithium cobalt oxide (such as LiCoO2 (LCO)) as an active material, carbon (such as carbon black, etc.) as a conductive material, and polyvinylidene fluoride (PVdF, etc.) as a binder with N-methylpyrrolidone (NMP) on a sheet-shaped current collector of aluminum foil; drying in a vacuum oven at about 120°C to manufacture a positive electrode sheet; and punching the positive electrode plate into a predetermined size.
[0047] The positive electrode waste has an active material layer on a current collector of a metal foil such as an aluminum foil. The active material layer is formed by applying a slurry including a mixture of an active material, a conductive material, a binder, and a solvent, and after the solvent is volatilized, the active material and the conductive material are combined with the binder. Therefore, when the binder is removed, the active material can be separated from the current collector.
[0048] Subsequently, the positive electrode waste is milled into an appropriate size (S20). Milling refers to cutting or chopping the positive electrode waste into an appropriate size for disposal. After milling, the positive electrode waste is cut into, for example, 1 cm×1 cm. Various dry milling equipment can be used in the milling process, including a hand mill, a pin mill, a disc mill, a cutting mill and a hammer mill as well as a high-speed cutter.
[0049] Milling can be performed considering the characteristics required by the equipment used in the disposal and subsequent processes of the cathode waste. For example, when equipment that requires continuous processing is used to load and unload cathode waste, it is necessary to mill the oversized cathode waste to facilitate the movement of the cathode waste.
[0050] Subsequently, the cathode waste is heat-treated in air ( S30 ).
[0051] In the present disclosure, heat treatment is performed to thermally decompose the binder in the active material layer. The heat treatment may be performed at 300°C to 650°C and may be referred to as high temperature heat treatment. At a temperature below 300°C, it is difficult to remove the binder, making it impossible to separate the current collector, and at a temperature of 650°C or more, the current collector melts (Al melting point: 660°C), making it impossible to separate the current collector.
[0052] The heat treatment time is long enough to cause the binder to thermally decompose. For example, the heat treatment time is about 30 minutes. Preferably, the heat treatment time is more than 30 minutes. As the heat treatment time increases, the thermal decomposition time of the binder will be extended, but when the heat treatment time is equal to or longer than the predetermined time, there is no difference in the thermal decomposition effect. Preferably, the heat treatment time is more than 30 minutes and less than 5 hours.
[0053] The heat treatment equipment may include various types of furnaces. For example, the heat treatment equipment may be a box-type furnace, and in consideration of productivity, may be a rotary kiln capable of continuous treatment.
[0054] After heat treatment, the product can be cooled quickly or slowly in air.
[0055] For example, the heat treatment may be performed at 550°C for 30 minutes with a temperature rise rate of 5°C / minute. For example, this temperature rise rate is within the allowable range of the box furnace and is sufficient to heat the positive electrode waste without generating thermal shock. 550°C is set in consideration of the melting point of the aluminum current collector and for good thermal decomposition of the binder. When the heat treatment is performed at the above temperature for less than 10 minutes, the thermal decomposition is insufficient, so it is necessary to perform the heat treatment for 10 minutes or longer, preferably 30 minutes or more.
[0056] Through the heat treatment in air, the CO2 and H2O are removed by thermal decomposition of the binder and the conductive material in the active material layer. Since the binder is removed, the active material can be separated from the current collector, and the active material to be collected can be screened out in the form of powder. Therefore, the current collector can be separated from the active material layer, and the active material in the active material layer can be collected by S30.
[0057] It is important to perform the heat treatment of S30 in air. When heat treated in a reducing atmosphere or an inert atmosphere, the binder and the conductive material undergo carbonization rather than thermal decomposition. When carbonized, carbon remains on the surface of the active material and degrades the performance of the reusable active material. When heat treated in air, the carbon in the binder or conductive material is removed by generating CO, CO2 gas through a combustion reaction with oxygen, so the binder and the conductive material do not remain and most of them are removed.
[0058] Therefore, according to the present disclosure, the active material is collected in the form of powder, and carbon generated by carbonization of the binder or the conductive material may not remain on the surface.
[0059] Subsequently, the collected active material is washed and dried (S40). It is important to wash with a lithium compound solution that is alkaline in an aqueous solution. The lithium compound solution contains a lithium compound, preferably LiOH, in an amount of more than 0% and less than 15%. Preferably, less than 15% LiOH is used. When an excess of LiOH is included, the excess LiOH may remain on the surface of the active material after washing, which may affect the subsequent annealing process. In order to make the surface of the active material as clean as possible before annealing, it is not advisable to add excess LiOH, and the amount of LiOH is limited to less than 15%.
[0060] The collected active material can be washed by soaking it in a lithium compound solution. Washing can be performed within a week after soaking, preferably one day, and more preferably 1 hour. When washing is performed for a week or longer, the capacity may decrease due to the dissolution of lithium. Therefore, it is best to wash within 1 hour. Washing includes soaking the active material in an alkaline lithium compound solution in an aqueous solution and stirring it while soaking. It is best to soak and stir together. When the active material is soaked in a lithium compound solution without stirring, the washing process is very slow, resulting in lithium dissolution. When stirring is performed together, the process time is minimized, therefore, it is best to stir while soaking in the lithium compound solution. It can be dried in an oven (convection type) in air after filtering.
[0061] Washing is performed with a lithium compound solution that is alkaline in an aqueous solution to remove LiF and metal fluorides that may be present on the surface of the collected active material, and surface modification is performed. During the heat treatment process of S30, the binder and the conductive material in the active material layer are removed by evaporation of CO2 and H2O, and in this process, CO2 and H2O react with the lithium on the surface of the active material to produce Li2CO3 and LiOH, while F (such as PVdF) present in the binder reacts with the metal element of the positive electrode active material to produce LiF or metal fluorides. When LiF or metal fluorides remain, the characteristics of the battery including the reusable active material will decrease. The present disclosure adds a washing step S40 to remove the reaction products that may be produced on the surface of the reusable active material in the heat treatment step (S30), thereby preventing impurities from remaining on the surface of the reusable active material.
[0062] In S40, it is important to wash with a lithium compound solution that is alkaline in aqueous solution. When sulfuric acid or hydrochloric acid aqueous solution is used instead of a lithium compound solution that is alkaline in aqueous solution, F on the surface of the active material is washed away, but the performance of the reusable positive active material may be reduced due to the dissolution of transition metals (Co, Mg) present in the active material. The role of the lithium compound solution that is alkaline in aqueous solution used in the present disclosure is to remove trace amounts of binders that may remain after the thermal decomposition of S30, not to dissolve transition metals present in the active material, and to compensate for the amount of lithium dissolved during the washing process.
[0063] Subsequently, annealing is performed by adding a lithium precursor to the washed active material (S50). S50 obtains a reusable active material.
[0064] The loss of lithium in the active material may occur through the previous steps S30 and S40. S50 compensates for the loss of lithium.
[0065] In addition, S50 restores the crystal structure of the active material through annealing, so that the properties of the reusable active material can be restored or improved to the level of fresh active material.
[0066] After the previous steps S30 and S40, the surface structure of the active material may be deformed. In addition, in the case of LCO active materials, Co3O4 may be generated on the surface by thermal decomposition. When the battery is manufactured, if Co3O4 is left on the surface, the battery characteristics may be reduced. The present disclosure can restore the crystal structure and remove Co3O4 by means of S50, thereby restoring or improving the initial characteristics to a level similar to that of fresh active materials.
[0067] The lithium precursor in S50 may be at least one of LiOH, Li2CO3, LiNO3 and Li2O.
[0068] The amount of lithium precursor added is used to add lithium to the ratio between lithium and other metals in the original active material (i.e., fresh active material) used in the active material layer at the ratio of lithium loss. For example, the ratio between lithium and other metals in the fresh active material is 1, and the amount of lithium precursor added can be used to add lithium at a molar ratio of 0.001 to 0.4. It is suitable to add lithium at a molar ratio of 0.01 to 0.2. The addition of lithium precursor exceeds the lithium loss caused by washing, which will leave unreacted lithium precursor on the reusable active material, resulting in increased resistance during the reuse of the active material. Therefore, it is necessary to add the lithium precursor in an appropriate amount.
[0069] Annealing can be performed in air at 400°C to 1000°C. The annealing temperature can be 600°C to 900°C. The temperature varies within a limited range, depending on the type of lithium precursor. The annealing time can be at least 1 hour. Preferably, the annealing time is about 5 hours. When the annealing time is long, the crystal structure may be fully restored, but long-term annealing does not have a great effect on the performance. For example, the annealing time is about 15 hours or less. The annealing equipment can be similar to or the same as the equipment of the heat treatment step S30.
[0070] For example, when Li2CO3 is used as a lithium precursor, the annealing temperature is preferably 700°C to 900°C, more preferably 710°C to 780°C. This is because the melting point of Li2CO3 is 723°C. Most preferably, annealing is performed at 750°C. When LiOH is used as a lithium precursor, the annealing temperature is preferably 400°C to 600°C, more preferably 450°C to 480°C. This is because the melting point of LiOH is 462°C.
[0071] Preferably, the annealing temperature is higher than the melting point of the lithium precursor. However, at a temperature higher than 1000°C, the positive electrode active material will undergo thermal decomposition and the performance of the active material will decrease. Therefore, the annealing temperature should not exceed 1000°C.
[0072] According to the present disclosure, LiF or metal fluoride is removed in the washing step of S40, and Co3O4 is removed in the annealing step of S50. The steps of washing and drying using a lithium compound solution that is alkaline in an aqueous solution are safe and low-cost, and can remove LiF or metal fluoride without losing other elements, prevent the dissolution of transition metals, and compensate for the lithium loss that occurs during the process. The annealing step is also safe and low-cost, and can effectively remove Co3O4 and restore the crystal structure (i.e., improve crystallinity), thereby improving the battery characteristics of the reusable active material.
[0073] The reusable active material obtained according to the present disclosure can have a similar particle size distribution as the active material in the active material layer present in the positive electrode waste, and does not need to be treated separately. Since the carbon generated by the carbonization of the binder or the conductive material does not remain on the surface, there is no need to perform a carbon removal step. Figure 2 The active material obtained by the method can be used to manufacture the positive electrode without any treatment.
[0074] The recycled active material may be used 100% without composition adjustment or may be mixed with fresh LCO and may be used to prepare a slurry together with a conductive material, a binder, and a solvent.
[0075] Hereinafter, experimental examples of the present disclosure will be described in detail.
[0076] <Experimental Example>
[0077] The positive electrode active materials were prepared by the methods of the following examples and comparative examples to evaluate the electrochemical performance.
[0078] Embodiment: Reusable active materials are collected according to the active material recycling method of the present disclosure as described above. Positive electrode waste discarded after positive plate stamping is prepared and heat-treated at 550°C for 30 minutes in S30. Washing of S40 is performed using LiOH for 10 minutes. In S50, annealing is performed at 750°C for 15 hours, and the amount of lithium precursor (Li2CO3) added is 2 mol% in excess of the lithium in the reusable LCO.
[0079] Comparative Example 1: Fresh LCO was used instead of the recyclable active material.
[0080] Comparative Example 2: As described above, in the active material recycling method of the present invention, by performing only the heat treatment of S30, the binder and the conductive material can be removed, the aluminum current collector can be separated, and the LCO active material can be collected. S30 is performed under the same conditions as in the embodiment. In the active material recycling method of the present invention, the surface modification of S40 and the crystal structure recovery of S50 are not performed.
[0081] Comparative Example 3: On the basis of Comparative Example 2, LCO active material was collected by performing surface modification of S40 in the active material recycling method of the present disclosure as described above. That is, surface modification was performed, but crystal structure recovery of S50 in the active material recycling method of the present disclosure was not performed. S40 was performed under the same conditions as in the embodiment.
[0082] 96 wt % of the positive electrode active material collected or prepared in the embodiments and comparative examples, 2 wt % of carbon black as a conductive material and 2 wt % of PVdF as a binder were measured and mixed with NMP to prepare a slurry, a positive electrode was made, a battery (Coin Half Cell, CHC) was manufactured and the electrochemical performance was evaluated.
[0083] Figure 3 Results of battery evaluation using active materials of Examples and Comparative Examples are shown. Capacity as a function of cycle number was evaluated at different currents to determine rate performance. The equipment used for evaluation is a charge / discharge tester commonly used in laboratories. There are no differences depending on the measuring equipment or method. Figure 3 In the graph of , the horizontal axis represents the number of cycles, and the vertical axis represents the capacity.
[0084] The voltage was 3 V to 4.5 V, and the initial formation charge / discharge was performed at 0.2 C / 0.2 C. The electrolyte solution of the battery was a carbonate-based electrolyte solution, and included ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3:7, and additives were added.
[0085] refer to Figure 3 , the lowest rate performance was found in Comparative Example 2 including a recyclable active material that was not subjected to surface modification and crystal structure recovery according to the present disclosure. This is because the binder and the conductive material were removed during the high temperature heat treatment of S30, generating CO2 and H2O, which reacted with lithium on the surface of the positive active material to generate Li2CO3 and LiOH, which in turn reacted with F present in the binder to generate LiF or metal fluoride. In addition, the low battery characteristics are probably due to the presence of Co3O4 on the surface of LCO due to thermal decomposition.
[0086] Comparative Example 3 was surface-modified compared to Comparative Example 2. It was evaluated that Comparative Example 3 had better results than Comparative Example 2 because Comparative Example 3 removed the reaction product on the surface by washing.
[0087] Compared with Comparative Example 3, the embodiment is annealed. Annealing is performed with the addition of Li2CO3 to compensate for lithium loss during the collection of active materials and to restore crystallinity. Not only the compensation for lithium loss that occurs during the process, but also the modified structure of the surface of the active material during the recovery process and the reduction of Co3O4 to the LCO crystal structure produce better results than the initial characteristics of the fresh active material of Comparative Example 1. According to the present disclosure, it is possible to collect active materials at directly usable levels from positive electrode waste. Since no toxic and explosive solvents such as NMP, DMC, acetone and methanol are used, and simple and safe methods such as heat treatment, washing and drying, and annealing are used, it is suitable for large-scale production.
[0088] Figure 4 The XRD patterns of the active materials of the embodiments and comparative examples are shown. In the XRD pattern, the horizontal axis represents 2θ (Theta) (degrees, °), and the vertical axis represents intensity. The XRD pattern can be obtained using an X-ray diffractometer commonly used in laboratories. For example, a Rigaku X-ray diffractometer XG-2100 can be used for analysis. However, there is no difference depending on the measuring device or method.
[0089] Figure 4 (a) shows the XRD pattern of Comparative Example 1 (ie, fresh LCO). Figure 4 (b) is the XRD pattern of the active material of Comparative Example 2, and Figure 4 (c) is an XRD pattern of the active material of Comparative Example 3. When (b) and (c) are compared with (a), Co3O4 phase can be observed. That is, it can be seen that Co3O4 is generated on the surface of LCO during the heat treatment of S30.
[0090] Figure 4 (d) is the XRD pattern of the active material of the embodiment. When (c) is compared with (d), it can be seen that the Co3O4 phase disappears, and the crystal structure is restored to LCO by annealing of S50. From the position of the diffraction peak in the XRD pattern, the crystal structure of (d) is similar to that of (a). Therefore, it is verified that the embodiment of the present disclosure is restored to the level of the fresh active material of Comparative Example 1. According to the present disclosure, active materials at a level that can be directly reused can be collected from positive electrode waste.
[0091] Figure 5 It is a scanning electron microscope (SEM) photographic image of the active material of the embodiment and the comparative example. This SEM photographic image is taken using a SEM device commonly used in the laboratory. For example, HITACHI s-4200 can be used for imaging. However, there is no difference depending on the measuring device or method.
[0092] Figure 5 (a) is a SEM photographic image of fresh LCO of Comparative Example 1, and Figure 5(b) is a SEM photographic image of the reusable active material of the embodiment. It can be seen that the LCO collected in the embodiment shows the same shape as the fresh LCO. In addition, only LCO was observed, which reveals that the binder and the conductive material were removed during the high-temperature heat treatment. Therefore, it can be seen that the active material is separated from the current collector by heat treatment in the air, and almost no binder or conductive material remains on the surface of the active material. According to the present disclosure, it is possible to separate the current collector from the active material without using complex methods or harmful materials, thereby collecting the active material in an environmentally friendly manner. Since no acid is used, no neutralization process or wastewater treatment process is required, thereby achieving environmental mitigation and process cost reduction.
[0093] Figure 6 : is a particle size distribution diagram of the active materials of the examples and comparative examples. The particle size distribution can be obtained using a particle size analyzer commonly used in the laboratory. For example, the characterization can be performed using a Horiba LA 950V2 particle size analyzer. However, there is no difference depending on the measuring equipment or method. Figure 6 In FIG. 1 , the horizontal axis represents the particle size (μm), and the vertical axis represents the volume (%).
[0094] All active materials collected in Examples and Comparative Examples 2 and 3 have similar particle size distributions compared to the fresh LCO of Comparative Example 1. The particle size distributions are defined as similar when the difference in volume % of particles having the same particle size is within the range of + / -2%. According to the present disclosure, since the particle size distribution of the active material does not change and the initial characteristics are almost maintained, it is expected that the characteristics of the battery including the recycled active material will be at a similar level to those of the battery using the fresh active material.
[0095] According to the present disclosure, cathode waste can be reused using a simple, environmentally friendly and economical method, and a lithium secondary battery manufactured by reusing the prepared LCO cathode active material has no problem in terms of battery performance.
[0096] Although the present disclosure has been described herein with respect to limited embodiments and drawings, the present disclosure is not limited thereto, and it will be apparent to those skilled in the art that various modifications and changes may be made thereto within the technical aspects of the present disclosure and the scope of the appended claims and their equivalents.
[0097] This application claims the benefit of Korean Patent Application No. 10-2020-0062370 filed on May 25, 2020, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety.
Claims
1. A method for recycling positive electrode active materials, the method comprising the following steps: (a) heat-treating a positive electrode waste including a lithium cobalt oxide positive electrode active material layer on a current collector in air to thermally decompose a binder and a conductive material in the active material layer, so as to separate the current collector from the active material layer, and collect active materials in the active material layer; (b) washing the collected active material with a basic lithium compound solution in aqueous solution and drying it to remove LiF or metal fluoride produced in step (a); as well as (c) annealing the washed active material with the addition of a lithium precursor to obtain a reusable active material, The lithium compound solution is a LiOH solution, and the content of the lithium compound in the lithium compound solution is at most 15%.
2. The method for recycling positive electrode active materials according to claim 1, wherein: The heat treatment is performed at 300°C to 650°C.
3. The method for recycling positive electrode active materials according to claim 1, wherein: The washing was carried out within 1 hour.
4. The method for recycling positive electrode active materials according to claim 1, wherein: The washing is performed by stirring the collected active material while immersing in the lithium compound solution.
5. The method for recycling positive electrode active materials according to claim 1, wherein: The lithium precursor is at least one of LiOH, Li2CO3, LiNO3 and Li2O.
6. The method for recycling positive electrode active materials according to claim 1, wherein: The lithium precursor is added in an amount for adding lithium at a molar ratio of 0.001 to 0.
4.
7. The method for recycling positive electrode active materials according to claim 1, wherein: The annealing is performed in air at 400° C. to 1000° C.
8. The method for recycling positive electrode active materials according to claim 1, wherein: The annealing temperature exceeds the melting point of the lithium precursor.
9. The method for recycling positive electrode active materials according to claim 1, wherein: The active material in the active material layer is collected in a powder form, and carbon generated by carbonization of the binder or the conductive material does not remain on the surface.
10. The method for recycling positive electrode active materials according to claim 1, wherein: The recyclable active material has a similar particle size distribution as that of the active material in the active material layer.
11. A method for recycling positive electrode active materials, the method comprising the following steps: (a) heat treating a positive electrode waste material remaining after punching a positive electrode plate in a positive electrode including a lithium cobalt oxide positive electrode active material layer on a current collector at 300° C. to 650° C. in air, wherein the heat treatment is used to thermally decompose a binder and a conductive material in the active material layer to separate the current collector from the active material layer, and collect the active material in the active material layer; (b) washing the collected active material with a lithium compound solution and drying it to remove LiF or metal fluoride produced in step (a), wherein the lithium compound solution is alkaline in aqueous solution, the lithium compound solution is a LiOH solution and the content of lithium compound in the lithium compound solution is at most 15%; and (c) annealing the washed active material in air at 400° C. to 1000° C. with the addition of at least one of LiOH, Li 2 CO 3 , LiNO 3 and Li 2 O.
Citation Information
Patent Citations
Additives for polyolefin resins, polyolefin resin compositions, polyolefin synthetic fiber nonwoven fabrics, and methods for producing polyolefin synthetic fiber nonwoven fabrics
KR1020200062370A
Method for recovering positive electrode active material from lithium secondary battery
CN108448193A
Recovering method for lithium ion secondary battery positive defective material
CN1585180A
Method of fabricating cathode for lithium ion secondary battery by recycling cathode active material and lithium ion secondary battery fabricated thereby
US20130266855A1