A method for preparing 1-chloro-2,3,3-trifluoropropene

By using magnesium and aluminum as the main components in the preparation of 1-chloro-2,3,3-trifluoropropylene, combined with a gas phase one-step reaction method, the complex process and the catalyst is prone to carbon decompression in the prior art. The problem is that efficient and low-cost production has been achieved, and the selectivity and conversion rate of HCFO-1233yd have been significantly improved.

CN114560750BActive Publication Date: 2024-11-22JUHUA GROUP TECH CENT
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202210108319.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2024-11-22
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

The existing preparation method of 1-chloro-2,3,3-trifluoropropylene has problems such as complex process, easy carbon deposition and low selectivity of catalysts, especially in the gas phase method, the catalyst costs are high and easy to lose carbon. live.

Method used

The catalyst is made of magnesium and aluminum as the main components, supplemented by calcium, strontium, barium, chromium, nickel, zirconium, lanthanum and other auxiliary components, and 3-chloro-1,1,2,2-tetrahydrogen Fluoropropane undergoes catalytic reaction with N2, optimizes the catalyst preparation process to improve activity and life, and controls reaction conditions to achieve efficient production.

Benefits of technology

The production process has been significantly simplified, the activity and service life of the catalyst has been improved. The selectivity of HCFO-1233yd has reached more than 95%, and the conversion rate is more than 91.5%, which has reduced production costs and overcomes the difficulty of continuous production in the existing technology and The problem of high catalyst cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing 1-chloro-2,3,3-trifluoropropene. Under the action of a catalyst, a mixed gas of 3-chloro-1,1,2,2-tetrafluoropropane and N2 is subjected to a gas phase catalytic reaction to obtain 1-chloro-2,3,3-trifluoropropene. The catalyst is mainly composed of magnesium and aluminum, and one selected from calcium, strontium, barium, chromium, nickel, zirconium, and lanthanum is an auxiliary component. The molar ratio of magnesium to aluminum is 1:1-2, and the amount of the auxiliary component is 2-5% of the total molar amount of magnesium and aluminum. The molar ratio of 3-chloro-1,1,2,2-tetrafluoropropane to N2 is 0.5-5:1, the reaction temperature is 350-650°C, and the mixed gas residence time is 0.5-15s. The present invention has the advantages of simple process, low cost, good catalyst activity, long service life, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chlorofluoroolefins, and in particular to a method for preparing 1-chloro-2,3,3-trifluoropropene. Background Art

[0002] 1-Chloro-2,3,3-trifluoropropene (CHCl=CF-CHF2, HCFO-1233yd) has a low global warming potential (GWP) and can be used in cleaning agents, refrigerants, foaming agents and other fields. It mainly replaces 3,3-dichloro-1,1,1,2,2-pentafluoropropane (CF3CF2CHCl2, HCFC-225ca) and 1,3-dichloro-1,1,2,2,3-pentafluoropropane (CClF2CF2CClFH, HCFC-225cb).

[0003] Currently, there are two main preparation routes for HCFO-1233yd:

[0004] (1) 1,1,2,3,3-pentachloropropane (CHCl2CHClCHCl2) gas phase fluorination method

[0005] For example, CN112125776A discloses a method for preparing HCFO-1233yd by first converting 1,1,2,3,3-pentachloropropane fluoride into 1,2-dichloro-3,3-difluoropropene (CHCl=CCl-CHF2, HCFO-1232xd) using a chromium-containing solid catalyst; and then fluorinating it with hydrogen fluoride in the gas phase under the catalysis of a chromium-based catalyst as the main catalyst to prepare HCFO-1233yd. The advantages of this process route are that the raw materials are easily available and inexpensive, the conversion rate of 1,1,2,3,3-pentachloropropane is high, and continuous production is possible; the disadvantages are that the process route is long, the catalyst is easily deactivated by carbon deposition, and the selectivity of HCFO-1233yd is low. The selectivity of preparing HCFO-1233yd by fluorination of HCFO-1232xd is about 80%.

[0006] (2) Dehydrofluorination of 3-chloro-1,1,2,2-tetrafluoropropane (CHF2CF2CH2Cl, R244ca)

[0007] The dehydrofluorination method of 3-chloro-1,1,2,2-tetrafluoropropane is divided into a liquid phase method and a gas phase method. The disadvantages of the liquid phase method are low degree of continuity, long reaction time, and large amount of organic waste liquid; the disadvantages of the gas phase method are high catalyst cost and easy carbon deposition and deactivation.

[0008] For example, CN107848917A discloses a method for preparing HCFO-1233yd by liquid phase dehydrofluorination of R244ca under the action of alkali and phase transfer catalyst. The alkali used in the process is at least one of metal hydroxide, metal oxide or metal carbonate, and the phase transfer catalyst includes quaternary ammonium salt, quaternary phosphonium salt, etc.

[0009] For example, CN107250088A discloses a method for preparing HCFO-1233yd by catalyzing R244ca in liquid or gas phase. The liquid phase method uses Bronsted acid such as sulfonic acid and phosphoric acid as a catalyst, an organic base or an inorganic base as a promoter, and a phase transfer catalyst to promote the fusion of the two phases; the gas phase method uses Lewis acid catalysts such as aluminum oxide, chromium oxide, tin oxide, ferric chloride, aluminum fluoride, aluminum oxide fluoride, and chromium oxide fluoride. Summary of the invention

[0010] The purpose of the present invention is to provide a method for preparing 1-chloro-2,3,3-trifluoropropene with simple process, safety, environmental protection, good catalyst activity and long life in view of the deficiencies in the prior art.

[0011] In order to solve the above technical problems, the present invention is achieved through the following technical scheme: a method for preparing 1-chloro-2,3,3-trifluoropropene, in the presence of a catalyst, a mixed gas of 3-chloro-1,1,2,2-tetrafluoropropane and N2 is subjected to a gas-phase catalytic reaction to obtain 1-chloro-2,3,3-trifluoropropene, the catalyst having magnesium and aluminum as main components, one selected from calcium, strontium, barium, chromium, nickel, zirconium, and lanthanum as an auxiliary component, the molar ratio of magnesium to aluminum is 1:1-2, the amount of the auxiliary component is 2-5% of the total molar amount of magnesium and aluminum, the molar ratio of 3-chloro-1,1,2,2-tetrafluoropropane to N2 is 0.5-5:1, the reaction temperature is 350-650°C, and the residence time of the mixed gas is 0.5-15s.

[0012] Preferably, the molar ratio of 3-chloro-1,1,2,2-tetrafluoropropane to N2 is 1 to 2:1, the reaction temperature is 400 to 550°C, and the residence time of the mixed gas is 1.5 to 5s.

[0013] Preferably, the catalyst is activated with nitrogen at the reaction temperature for 2 to 6 hours before the reaction begins.

[0014] The catalyst described in the present invention is prepared by the following method:

[0015] (1) grinding and mixing aluminum, magnesium, a compound of an auxiliary component and ammonium fluoride in proportion to obtain a mixture;

[0016] (2) drying the mixture to obtain a dried product;

[0017] (3) calcining the dried product to obtain a catalyst.

[0018] Preferably, the compounds of aluminum, magnesium and auxiliary components are chlorides, nitrates and carbonates.

[0019] Preferably, the compound of the auxiliary component is a chloride.

[0020] Preferably, the amount of ammonium fluoride added is 1.2 to 2 times the total molar amount of fluoride ions required for all metal ions to form saturated fluoride.

[0021] Preferably, the grinding time is 25 to 45 minutes.

[0022] Preferably, the drying temperature is 110-150° C., the time is 5-15 hours, and the calcination temperature is 350-450° C., the time is 2-6 hours.

[0023] Preferably, the calcination temperature is 350-450° C. and the calcination time is 2-6 hours.

[0024] The catalyst used in the prior art gas phase catalytic R244ca preparation of HCFO-1233yd is mainly Al-based and Cr-based, and most of them are prepared by precipitation method. The catalyst has a small specific surface area, strong acidity and is easily deactivated by carbon deposition. The present invention adopts a solid phase grinding method to prepare a metal fluoride catalyst. The prepared catalyst has magnesium and aluminum as main components, and one selected from calcium, strontium, barium, chromium, nickel, zirconium and lanthanum as an auxiliary component. The main component provides the necessary active sites for the catalyst, and the auxiliary component has the function of adjusting the surface acidity of the main catalyst. The main component and the auxiliary component work synergistically, effectively improving the activity and service life of the catalyst, and has the advantages of simple process, low cost, good catalyst activity and long service life.

[0025] The grinding time in the present invention is preferably 25 to 45 minutes. By controlling the grinding time, the uniformity of the obtained product is improved, the specific surface area of ​​the catalyst is increased, and the carbon deposition rate of the catalyst is slowed down.

[0026] In the present invention, the molar ratio of magnesium to aluminum has a great influence on the number of active sites of the catalyst, and thus affects the conversion rate of the raw material. If the molar ratio is too large, the number of strong acid sites of the catalyst is reduced, which in turn affects the conversion rate of the raw material; if the molar ratio is too small, the number of strong acid sites increases, and the catalyst is prone to carbon deposition and deactivation. Therefore, the molar ratio of magnesium to aluminum in the present invention is preferably 1:1-2.

[0027] In the present invention, the amount of auxiliary components has an effect on adjusting the acidity of the main catalyst. If the amount of auxiliary components is too much, the surface acid sites of the main catalyst are easily covered by the auxiliary components; if the amount of auxiliary components is too little, they are easily wrapped in the catalyst body phase and cannot play a role in adjusting the surface acidity of the main catalyst. Therefore, the amount of auxiliary components in the present invention is preferably 2-5% of the total molar amount of magnesium and aluminum.

[0028] In the present invention, the drying temperature is preferably 110-150° C., and the drying time is preferably 5-15 hours. Controlling the drying temperature and time can effectively improve the uniformity of the catalyst, thereby further increasing the specific surface area of ​​the catalyst and slowing down the carbon deposition rate of the catalyst.

[0029] In the present invention, the calcination temperature is preferably 350-450° C., and the calcination time is preferably 2-6 hours. Controlling the calcination temperature and time can increase the surface acidity of the catalyst, thereby further improving the catalyst activity.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The process is simple and efficient. It adopts a gas-phase one-step reaction process with simple operation and mild reaction conditions, which significantly simplifies the production process and facilitates continuous production. It overcomes the shortcomings of the existing process, such as difficulty in continuous production, high catalyst cost, and easy carbonization and deactivation;

[0032] 2. The catalyst has good activity and long service life. The present invention adopts a solid phase grinding method to prepare the catalyst, and by optimizing the feed formula and process parameters, the specific surface area of ​​the catalyst is increased, the carbon deposition rate of the catalyst is delayed, and the service life and activity of the catalyst are effectively prolonged. The prepared catalyst has magnesium and aluminum as main components, and one selected from calcium, strontium, barium, chromium, nickel, zirconium, and lanthanum is an auxiliary component. The main component provides the necessary active sites for the catalyst, and the auxiliary component has the function of adjusting the surface acidity of the main catalyst. The main component and the auxiliary component work synergistically, which effectively improves the activity and service life of the catalyst. The selectivity of HCFO-1233yd is above 95%, and can reach up to 98% at the highest. The conversion rate of R244ca is above 91.5%, and can reach up to 95%.

[0033] 3. Low cost. The method for preparing HCFO-1233yd of the present invention adopts a gas phase one-step reaction process, which is simple in process; an aluminum-magnesium-based catalyst is used as a main catalyst, and the catalyst preparation method is simple and efficient, which significantly reduces the production cost. DETAILED DESCRIPTION

[0034] The invention is further described in detail below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.

[0035] Example 1

[0036] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 2:1 are added into a mortar, and then calcium chloride and ammonium fluoride are added. The amount of calcium chloride added is 2% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.2 times the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 30 minutes, put it into an oven and dry it at 110°C for 12 hours. The dried product is calcined at 450°C for 2 hours to obtain a catalyst.

[0037] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 500°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 500℃ for 5h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1:1 and introduced into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 3s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 96% and the conversion rate of R244ca was 91.5%.

[0038] Example 2

[0039] Aluminum nitrate and magnesium carbonate in a molar ratio of 2:1 are added to a mortar, and then strontium chloride and ammonium fluoride are added. The amount of strontium chloride added is 3% of the total molar amount of aluminum nitrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.3 times the molar amount of fluoride ions required for aluminum nitrate and magnesium carbonate to form saturated aluminum fluoride and magnesium fluoride. The mixture is ground for 35 minutes and then placed in an oven and dried at 120°C for 10 hours. The dried product is calcined at 430°C for 3 hours to obtain a catalyst.

[0040] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 450°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 450℃ for 4h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1.1:1 and passed into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 4s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 97.5% and the conversion rate of R244ca was 95%.

[0041] Example 3

[0042] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 1:1 are added into a mortar, and then barium chloride and ammonium fluoride are added. The amount of barium chloride added is 5% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.4 times the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 40 minutes, put it into an oven and dry it at 130°C for 9 hours. The dried product is calcined at 420°C for 4 hours to obtain a catalyst.

[0043] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 400°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 400℃ for 6h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1.2:1 and passed into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 3.5s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 98% and the conversion rate of R244ca was 93.5%.

[0044] Example 4

[0045] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 1.5:1 are added to a mortar, and then chromium chloride and ammonium fluoride are added. The amount of chromium chloride added is 4.5% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.5 times the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 45 minutes, put it into an oven and dry it at 140°C for 8 hours. The dried product is calcined at 450°C for 5 hours to obtain a catalyst.

[0046] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 400°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 400℃ for 2h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1.5:1 and passed into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 4.5s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 96% and the conversion rate of R244ca was 91.5%.

[0047] Example 5

[0048] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 1.6:1 are added to a mortar, and then nickel chloride and ammonium fluoride are added. The amount of nickel chloride added is 3.5% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.6 times the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 25 minutes, put it into an oven and dry it at 150°C for 7 hours. The dried product is calcined at 380°C for 5.5 hours to obtain a catalyst.

[0049] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 480°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 480℃ for 3h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1.6:1 and introduced into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 5s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 97% and the conversion rate of R244ca was 93.5%.

[0050] Example 6

[0051] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 1.7:1 are added to a mortar, and then zirconium chloride and ammonium fluoride are added. The amount of zirconium chloride added is 2.5% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is 1.7 times the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 30 minutes, put it into an oven and dry it at 125°C for 5 hours. The dried product is calcined at 370°C for 4 hours to obtain a catalyst.

[0052] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 490°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 490℃ for 4.5h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 1.8:1 and passed into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 1.5s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 98% and the conversion rate of R244ca was 94.5%.

[0053] Example 7

[0054] Aluminum chloride hexahydrate and magnesium chloride hexahydrate in a molar ratio of 1.8:1 are added to a mortar, and then lanthanum chloride and ammonium fluoride are added. The amount of lanthanum chloride added is 5% of the total molar amount of aluminum chloride hexahydrate and magnesium chloride hexahydrate, and the amount of ammonium fluoride added is twice the molar amount of fluoride ions required for aluminum chloride hexahydrate and magnesium chloride hexahydrate to form saturated aluminum fluoride and magnesium fluoride. After grinding the mixture for 35 minutes, put it into an oven and dry it at 135°C for 6 hours. The dried product is calcined at 350°C for 6 hours to obtain a catalyst.

[0055] The prepared catalyst was loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor was a 316L tube with an inner diameter of 10 mm and a length of 800 mm. The reactor was placed in a heating furnace and heated to 550°C for reaction. The reaction pressure was normal pressure. Before the reaction, N2 (space velocity of 1200 h -1 ) was activated at 550℃ for 4h. R244ca was then gasified at 80℃ and mixed with N2 at a molar ratio of 2:1 and introduced into a plug flow tubular reactor for gas phase catalytic reaction. The residence time of the mixed gas was 4.5s. The tail gas generated by the reaction was tested after rapid cooling, alkali washing, water washing and drying. Based on the consumption of R244ca, the selectivity of HCFO-1233yd was 98% and the conversion rate of R244ca was 94.5%.

Claims

1. A method for preparing 1-chloro-2,3,3-trifluoropropene, characterized in that: Aluminum nitrate and magnesium carbonate in a molar ratio of 2:1 are added to a mortar, and then strontium chloride and ammonium fluoride are added, wherein the amount of strontium chloride added is 3% of the total molar amount of aluminum nitrate and magnesium carbonate, and the amount of ammonium fluoride added is 1.3 times the molar amount of fluoride ions required for aluminum nitrate and magnesium carbonate to form saturated aluminum fluoride and magnesium fluoride. The mixture is ground for 35 minutes and then placed in an oven and dried at 120°C for 10 hours. The dried product is calcined at 430°C for 3 hours to obtain a catalyst. The prepared catalyst is loaded into a plug flow tubular reactor. The reaction tube of the plug flow tubular reactor adopts a 316L tube with an inner diameter of 10 mm and a length of 800 mm, and is placed in a heating furnace and heated to 450°C for reaction. The reaction pressure is normal pressure. Before the reaction, a space velocity of 1200 h is introduced. -1 The N2 was activated at 450°C for 4h, and then 3-chloro-1,1,2,2-tetrafluoropropane was gasified at 80°C and mixed with N2 at a molar ratio of 1.1:

1. The mixture was introduced into a plug flow tubular reactor for a gas phase catalytic reaction. The residence time of the mixed gas was 4s to obtain 1-chloro-2,3,3-trifluoropropene.

Citation Information

Patent Citations

  • Method for producing 1-chloro-2,3,3-trifluoropropene

    CN107250088A

  • Method for producing 1-chloro-2,3,3-trifluoropropene

    CN107848917A

  • Preparation method of 1-chloro-2, 3, 3-trifluoropropene

    CN112125776A

  • Method for preparing fluorinated alkene by performing dehydrochlorination on chlorofluorocarbon under action of catalyst

    CN103420782A

  • Catalyst for preparing trifluoroethylene

    CN103861579A