Polymer dispersion and preparation method thereof, polymer composite membrane and application thereof

By mixing the liquid crystal polymer powder with polyamic acid containing liquid crystal structure and flexible structure to form a polymer composite film, the signal transmission loss and electron transmission instability caused by dielectric layer materials are solved, and the polymer composite film is realized Good adhesion and mechanical performance improvement.

CN114561029BActive Publication Date: 2024-11-08ZHEN DING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011365021.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-11-08
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

The dielectric layer materials in existing printed circuit boards lead to signal transmission losses and electronic transmission instability, especially the process limitations and difficulties of liquid crystal polymer materials in the film formation and copper clad production process.

Method used

Using a polymer dispersion liquid, including liquid crystal polymer powder and polyamic acid, the polymer composite film is formed by mixing the liquid crystal polymer powder with polyamic acid containing liquid crystal structure and flexible structure, and the network structure is reduced. Dielectric loss and thermal expansion coefficient improve mechanical properties.

Benefits of technology

It effectively improves the solid content and viscosity of the dispersion liquid, has good stability, and has good adhesion between the polymer composite film and copper plate, which reduces dielectric loss and thermal expansion coefficient, and improves mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114561029B_ABST
    Figure CN114561029B_ABST
Patent Text Reader

Abstract

A polymer dispersion liquid and a preparation method thereof, a polymer composite film and an application thereof, wherein the polymer dispersion liquid comprises liquid crystal polymer powder, polyamic acid and a solvent, the solid components of the polymer dispersion liquid comprise polyamic acid and liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid components of the polymer dispersion liquid is 20% to 30%, the weight percentage of the polyamic acid in the solid components of the polymer dispersion liquid is 70% to 80%, and the polyamic acid is polymerized by two diamine monomers and two dianhydride monomers, and the two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure. The polymer dispersion liquid provided by the present invention can effectively increase the solid content and viscosity of the dispersion liquid, and is conducive to film formation; the formed copper clad laminate has excellent electrical and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer material preparation, and in particular to a method for preparing a polymer dispersion, a polymer composite film and applications thereof. Background Art

[0002] The signal transmission loss in the printed circuit board is partly due to the loss caused by the dielectric layer. The loss caused by the dielectric layer is usually related to the dielectric constant and dielectric loss factor of the dielectric layer material. In addition, the polarity of the dielectric layer material will affect the stability of electron transmission in the wire. If the polarity of the molecular structure in the insulating layer material is too large, after the circuit board is polarized, the electrons in the wire will be attracted by the dielectric layer, which will seriously affect the stability of electron transmission. Therefore, how to effectively design the polymer structure of the dielectric layer, reduce the dielectric loss of the dielectric layer polymer material, and achieve a good insulation effect will become an important topic.

[0003] At present, liquid crystal polymer (LCP) materials are widely used in printed circuit boards because of their liquid crystal structure and low dielectric loss. However, LCP materials have low solid content and viscosity, and need to be formed into films without solvents and at high temperatures. The film-forming process has many restrictions, and it is also difficult to press the film with the copper plate to make a copper-clad laminate after film formation. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a polymer dispersion and a preparation method thereof.

[0005] In addition, the present invention also provides a polymer composite membrane prepared from the polymer dispersion and its application.

[0006] The invention provides a polymer dispersion liquid, comprising liquid crystal polymer powder, polyamic acid and a solvent. The solid components of the polymer dispersion liquid include the polyamic acid and the liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid components of the polymer dispersion liquid is 20% to 30%, the weight percentage of the polyamic acid in the solid components of the polymer dispersion liquid is 70% to 80%, and the polyamic acid is polymerized by two diamine monomers and two dianhydride monomers, and the two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure.

[0007] In the embodiment of the present application, the particle size of the liquid crystal polymer powder is less than or equal to 3 μm.

[0008] In the embodiment of the present application, the solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40,000 cps to 50,000 cps.

[0009] In the embodiment of the present application, the liquid crystal polymer powder includes aromatic liquid crystal polyester.

[0010] The present invention also provides a method for preparing a polymer dispersion, comprising the following steps:

[0011] A polyamic acid solution is provided, which comprises polyamic acid and a solvent. The polyamic acid is polymerized by two diamine monomers and two dianhydride monomers. The two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure.

[0012] And, liquid crystal polymer powder is added into the polyamic acid solution, and mixed to obtain the polymer dispersion.

[0013] The solid component of the polymer dispersion includes the polyamic acid and the liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid component of the polymer dispersion is 20% to 30%, and the weight percentage of the polyamic acid in the solid component of the polymer dispersion is 70% to 80%.

[0014] In the embodiment of the present application, the average particle size of the liquid crystal polymer powder is less than or equal to 3 μm.

[0015] In the embodiment of the present application, the solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40,000 cps to 50,000 cps.

[0016] In the embodiment of the present application, the liquid crystal polymer powder includes aromatic liquid crystal polyester.

[0017] In the embodiment of the present application, the diamine monomer containing a liquid crystal structure includes one or more of p-aminophenyl p-aminobenzoate, 1,4-bis(4-aminophenoxy)benzene and di-p-aminophenyl terephthalate.

[0018] The diamine monomer containing a flexible structure includes one or more of 4,4'-diaminodiphenyl ether, 2,2'-bis[4-(4-aminophenoxyphenyl)]propane, 1,3-bis(4'-aminophenoxy)benzene and 1,3-bis(3-aminophenoxy)benzene.

[0019] In the embodiment of the present application, the dianhydride monomer containing a liquid crystal structure includes 3,3',4,4'-biphenyltetracarboxylic dianhydride, p-phenylene bis(trimellitate) dianhydride and cyclohexane-1,4-diylbis(methylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid ethyl ester).

[0020] The dianhydride monomer containing a flexible structure includes one or more of 4,4'-oxydiphthalic anhydride and bisphenol A diether dianhydride.

[0021] The present invention also provides a polymer composite film, which is obtained by heating the polymer dispersion as described above, and comprises liquid crystal polymer crystals and polyimide crystals, and the liquid crystal polymer crystals and the polyimide crystals are cross-linked to form a network structure.

[0022] In the implementation manner of the present application, the weight percentage of the liquid crystal polymer crystals in the polymer composite film is 20% to 30%.

[0023] In the embodiment of the present application, the polymer composite film is an anisotropic thermoplastic film.

[0024] The present invention also provides a copper-clad laminate comprising a copper foil and a polymer composite film laminated on at least one surface of the copper foil, wherein the polymer composite film comprises the polymer composite film as described above.

[0025] Compared with the prior art, the polymer dispersion provided by the present invention forms a dispersion by mixing liquid crystal polymer powder with thermoplastic polyamic acid containing both a liquid crystal structure and a flexible structure, which can effectively improve the solid content and viscosity of the dispersion, and the formed dispersion has good stability, which is conducive to the film formation of the dispersion, and the formed polymer composite film in the copper clad laminate has good adhesion to the copper plate, and at the same time, the two crystal phases formed in the polymer composite film can form a network structure through crystallization cross-linking points, which effectively reduces the Df and thermal expansion coefficient of the copper clad laminate, and at the same time improves the mechanical properties of the polymer composite film. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1A-1B It is a schematic diagram of crystallization of a polymer dispersion during heating provided by one embodiment of the present invention.

[0027] Figure 2A-2C It is a preparation flow chart of a copper clad laminate provided in one embodiment of the present invention.

[0028] Main component symbols

[0029] Copper Clad Laminate 100 Copper Plate 10 Polymer composite membrane 20 Polymer dispersion film 30 Liquid crystal polymer crystal 1 Polyamic acid molecule 2 Polyimide crystal 3

[0030] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described implementation is only a part of the implementation of the present invention, not all of the implementations. Based on the implementation of the present invention, all other implementations obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The names of the technical means used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0033] In the absence of conflict, the following embodiments and features of the embodiments may be combined with each other.

[0034] The present invention provides a polymer dispersion liquid, which comprises liquid crystal polymer powder (LCP powder), polyamic acid and solvent, wherein the solid components of the polymer dispersion liquid comprise the polyamic acid and the liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid components of the polymer dispersion liquid is 20% to 30%, and the weight percentage of the polyamic acid in the solid components of the polymer dispersion liquid is 70% to 80%. The polyamic acid is polymerized by two diamine monomers and two dianhydride monomers, and the two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure.

[0035] In this embodiment, the average particle size of the liquid crystal polymer powder is less than or equal to 3 μm.

[0036] In this embodiment, the solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40000 cps to 50000 cps. By adding liquid crystal polymer powder, the liquid crystal polymer powder is insoluble but dispersible in the solvent, so the viscosity of the polymer dispersion can be effectively increased, thereby improving the stability of the dispersion and facilitating subsequent film formation.

[0037] In this embodiment, the liquid crystal polymer powder includes but is not limited to aromatic liquid crystal polyester.

[0038] In this embodiment, the solvent includes but is not limited to N-methylpyrrolidone (NMP).

[0039] The present invention also provides a method for preparing a polymer dispersion, comprising the following steps:

[0040] The first step is to synthesize a polyamic acid solution.

[0041] The polyamic acid is polymerized by two diamine monomers and two dianhydride monomers, and the two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure.

[0042] In this embodiment, the diamine monomer containing a liquid crystal structure includes, but is not limited to, one or more of p-aminophenyl para-aminobenzoate (APAB), 1,4-bis(4-aminophenoxy)benzene (ABHQ), and di-p-aminophenyl terephthalate (BPTP). The diamine monomer containing a flexible structure includes, but is not limited to, one or more of 4,4'-diaminodiphenyl ether (ODA), 2,2'-bis[4-(4-aminophenoxyphenyl)]propane (BAPP), 1,3-bis(4'-aminophenoxy)benzene (TPE-R), and 1,3-bis(3-aminophenoxy)benzene (TPE-M).

[0043] In this embodiment, the dianhydride monomer containing a liquid crystal structure includes, but is not limited to, one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), p-phenylene bis(trimellitate) dianhydride (TAHQ), and cyclohexane-1,4-diylbis(methylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid ethyl ester) (TA-CHDM). The dianhydride monomer containing a flexible structure includes, but is not limited to, one or more of 4,4'-oxydiphthalic anhydride (ODPA) and bisphenol A diether dianhydride (BPADA).

[0044] In this embodiment, the combination of diamine and dianhydride in the four monomers is random, and the obtained polyamic acid is a mixture of polyamic acids with a series of different molecular structures. Specifically, the structural formula of a specific product obtained by using diamines such as APAB and TPE-R and dianhydrides such as TAHQ and BPADA is given below as an example:

[0045] Structural Formula I:

[0046]

[0047] Structural formula II:

[0048]

[0049] Structural formula III:

[0050]

[0051] In this embodiment, the addition ratio of the diamine monomer to the dianhydride monomer is preferably 1:1.

[0052] In this embodiment, the solvent includes but is not limited to N-methylpyrrolidone (NMP).

[0053] In this embodiment, the diamine monomer and the dianhydride monomer react at room temperature for about 48 hours to generate a polyamic acid block copolymer. The solid content of the polyamic acid solution is 20 wt% to 30 wt%.

[0054] In the second step, the liquid crystal polymer powder is added to the polyamic acid solution and mixed to obtain the polymer dispersion. The solid components of the polymer dispersion include the polyamic acid and the liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid components of the polymer dispersion is 20% to 30%, and the weight percentage of the polyamic acid in the solid components of the polymer dispersion is 70% to 80%.

[0055] In this embodiment, the particles of the liquid crystal polymer powder are added to the polyamic acid solution, and the liquid crystal polymer powder is insoluble but can be evenly dispersed in the solution to form the polymer dispersion. The average particle size of the liquid crystal polymer powder is less than or equal to 3 μm. The liquid crystal polymer powder of this size can better contact with the polyamic acid, increase the contact area between the two, and is conducive to the uniform dispersion of the powder particles in the polymer dispersion, which is convenient for subsequent coating and film formation. If the average particle size of the liquid crystal polymer powder is too large, the polymer dispersion is prone to sedimentation, and uneven thickness is prone to occur during subsequent coating and film formation, and the large particles of the liquid crystal polymer powder cannot fully contact with the polyamic acid, resulting in subsequent inability to form a homogeneous film.

[0056] In this embodiment, the solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40000 cps to 50000 cps. By adding liquid crystal polymer powder to the thermoplastic polyamic acid solution to form a uniformly mixed dispersion, the solid content and viscosity of the dispersion can be effectively increased, which is beneficial to subsequent film formation.

[0057] In this embodiment, the liquid crystal polymer powder includes but is not limited to aromatic liquid crystal polyester.

[0058] The present invention also provides a polymer composite film, which is prepared by heating the polymer dispersion as described above. Figure 1A-1B In the process of heating and curing the dispersion to form a film, the liquid crystal polymer crystal 1 corresponding to the liquid crystal polymer powder melts to form a flowable melt, and the polyamic acid molecule 2 is heated and cyclized to form a polyimide melt. The liquid crystal polymer melt is evenly distributed in the polyimide melt, such as Figure 1A As shown. The liquid crystal polymer powder has a liquid crystal structure (ester group), and the polyimide also contains a liquid crystal structure (ester group). Both can crystallize during the cooling process. The liquid crystal polymer melt recrystallizes to form a liquid crystal polymer crystal 1 again, and the polyimide crystallizes to form a polyimide crystal 3. Figure 1B As shown. Since the two melts are uniformly mixed together, the two crystalline phases will also form a large number of physical crystal crosslinking points, which connect the liquid crystal polymer crystalline phase and the polyimide crystalline phase together to form a network structure, such as Figure 1BIn the structure of the enlarged figure, the liquid crystal polymer crystal 1 and the polyimide crystal 3 are interlaced to form a physical crystalline cross-linked network structure. The formed network structure effectively improves the mechanical properties of the polymer composite film, while reducing the thermal expansion coefficient (CTE) of the polymer composite film, thereby improving the dimensional stability of the polymer composite film. In addition, when forming a polymer dispersion, since the liquid crystal polymer powder is evenly distributed in the polyamic acid solution, and the average particle size of the liquid crystal polymer powder is very small, during the heating film forming process, the liquid crystal polymer powder can be fully melted to form a uniform mixed melt with the polyimide melt. After the two melts are crystallized, two crystals are formed, and the two crystals are cross-mixed to form a network structure, and the arrangement direction of the two crystals is anisotropic, thereby giving the polymer composite film anisotropic characteristics.

[0059] In this embodiment, the average particle size of the liquid crystal polymer powder is less than or equal to 3 μm. In the process of forming the dispersion, the liquid crystal polymer powder of this size can better contact with the polyamic acid, increase the contact area between the two, and at the same time help to increase the viscosity of the polymer dispersion, which is convenient for coating the polymer dispersion into a film. When the average particle size of the liquid crystal polymer powder is too large, the polymer dispersion is prone to sedimentation, and the thickness is prone to unevenness during subsequent coating and film formation. Moreover, when melting at high temperature, the liquid crystal polymer powder particles with a particle size greater than 3 μm cannot be completely melted, resulting in the inability to form a homogeneous film.

[0060] In this embodiment, the proportion of the two crystals can be adjusted by adjusting the content of the liquid crystal polymer powder and the polyamic acid, thereby adjusting the mechanical properties and electrical properties of the composite film. In addition, the mechanical properties and electrical properties of the composite film can be further adjusted by adjusting the introduction of the liquid crystal structure during the synthesis of the polyamic acid.

[0061] In this embodiment, the weight percentage of the liquid crystal polymer crystals 1 in the polymer composite film is 20% to 30% of the polymer composite film.

[0062] In this embodiment, the heating temperature is 350° C. to 370° C., and the heating time is 30 min to 60 min. The specific heating temperature may vary according to the glass transition temperature of the actual polymer dispersion.

[0063] In this embodiment, the thermal expansion coefficient of the polymer composite film is less than or equal to 45 ppm / ° C., the tensile strength is greater than or equal to 130 MPa, and the elongation is greater than or equal to 18%.

[0064] Specifically, the film-forming process of the polymer composite film is as follows: coating the polymer dispersion with a thickness of greater than or equal to 50 μm on a release substrate, and then passing the release substrate coated with the polymer dispersion film layer through an oven for baking and heating, usually at 350° C. to 370° C. for 30 min to 60 min, to obtain the polymer composite film. At the above temperature, the liquid crystal polymer powder particles will melt and become a melt, which can better form a homogeneous film.

[0065] See also Figure 2A-2C The present invention also provides a preparation process of a copper clad laminate 100, which specifically includes the following steps:

[0066] See also Figure 2A , a copper foil 10 is provided, and the thickness of the copper foil 10 can be selected according to actual use requirements. Specifically, in this embodiment, the thickness of the copper foil 10 is 12 μm.

[0067] See also Figure 2B The polymer dispersion is coated on one surface of the copper foil 10 to form a polymer dispersion film 30 to obtain an intermediate. Specifically, in this embodiment, the thickness of the polymer dispersion film 30 is 50 μm.

[0068] See also Figure 2C , the intermediate is placed in an oven for heating, so that the polymer dispersion film 30 is cured to form a polymer composite film 20, thereby obtaining the copper clad laminate 100. In this embodiment, the polymer dispersion film 30 is heated at 350°C to 370°C for 30min to 60min to obtain the polymer composite film 20.

[0069] The copper clad laminate 100 includes a copper foil 10 and a polymer composite film 20 laminated on the surface of the copper foil 10 . The polymer composite film 20 is the polymer composite film as described above.

[0070] In this embodiment, the copper clad laminate 100 has excellent electrical properties. Electrical performance tests are performed at a frequency of 10 GHz, and it can be seen that the copper clad laminate has excellent dielectric loss factor (Df) and dielectric constant (Dk), wherein Dk is preferably 3.3 to 3.2, and Df is preferably 0.002 to 0.001.

[0071] In this embodiment, the peel strength of the polymer composite film 20 on the surface of the copper foil 10 is preferably greater than or equal to 0.7 kgf / cm. In the heat resistance test, the polymer composite film has good heat resistance at 288°C / 10sec.

[0072] In addition, a double-sided copper clad laminate can also be prepared by the above method.

[0073] The present invention also provides another method for preparing a copper clad laminate, first preparing a polymer composite film, and then laminating the polymer composite film on at least one side of a copper foil and performing hot pressing to form the copper clad laminate. The specific conditions for hot pressing laminating are: a hot pressing temperature of 350°C to 370°C, and a pressure per unit area of ​​30 to 80 kgf / mm 2 , the hot pressing agent is within 10 to 30 minutes. Specifically, a single-sided or double-sided copper-clad laminate can be prepared by this method. The scheme of the present application is further described below through specific embodiments.

[0074] The following synthesis examples 1-5 are all specific synthesis methods of polyamic acid solutions, and the solid content of the synthesized polyamic acid solutions is 20wt% to 30wt%. After the polyamic acid solution is synthesized, a 50μm thick polyamic acid solution is coated on a 12μm copper plate, and baked at 350℃ to 370℃ for 30min to 60min, the solvent is removed and the polyamic acid is cyclized to form polyimide and melted, and then cooled to form a polyimide film, thereby obtaining a copper clad laminate, and the above copper clad laminate is tested for mechanical properties and electrical properties.

[0075] Synthesis example 1

[0076] In a 500 mL reaction bottle, NMP (243.8 g) and TPE-M (0.1 mol, 29.23 g) were added respectively, and after stirring until dissolved, BPADA (0.1 mol, 52.05 g) was added and stirred for reaction for 48 hours to complete the preparation of the polyamic acid solution.

[0077] Synthesis example 2

[0078] In a 500 mL reaction bottle, NMP (205.97 g) and APAB (0.1 mol, 22.83 g) were added respectively, and after stirring until dissolved, TAHQ (0.1 mol, 45.83 g) was added and stirred for reaction for 48 hours to complete the preparation of the polyamic acid solution.

[0079] Synthesis example 3

[0080] In a 500 mL reaction bottle, NMP (225.20 g) and TPE-M (0.1 mol, 29.2 g) were added respectively, and after stirring until dissolved, TAHQ (0.1 mol, 45.83 g) was added and stirred for reaction for 48 hours to complete the preparation of the polyamic acid solution.

[0081] Synthesis example 4

[0082] In a 500 mL reaction bottle, NMP (224.62 g) and APAB (0.1 mol, 22.83 g) were added respectively, and after stirring until dissolved, BPADA (0.1 mol, 52.05 g) was added and stirred for reaction for 48 hours to complete the preparation of the polyamic acid solution.

[0083] Synthesis example 5

[0084] In a 500mL reaction bottle, NMP (224.91g) and TPE-M (0.05mol, 14.61g) were added respectively. After stirring until dissolved, TAHQ (0.05mol, 22.93g) was added and stirred for reaction for 1 hour. Then, APAB (0.05mol, 11.41g) was added. After stirring until dissolved, BPADA (0.05mol, 26.02g) was added and stirred for reaction for 48 hours. The polyamic acid solution was thus prepared.

[0085] The specific ratios of the raw materials for preparing polyamic acid and the test results of the corresponding copper clad laminates are shown in Table 1.

[0086] Table 1

[0087]

[0088]

[0089] Note: Ts is the thermal processing temperature of polyimide, where Ts is between the glass transition temperature Tg and the melting temperature Tm.

[0090] The following examples 1-3 are all specific synthesis methods of polymer dispersions, and the solid content of the synthesized polymer dispersions is 25wt% to 35wt%. After the polymer dispersion is synthesized, the polymer dispersion is coated on a 12μm copper plate with a thickness of 50μm, and baked at 350℃ to 370℃ for 30min to 60min to remove the solvent and melt the polyimide and liquid crystal polymer powders, and then cooled to form a polymer composite film, thereby obtaining a copper clad laminate, and the mechanical properties and electrical properties of the copper clad laminate are tested.

[0091] Example 1

[0092] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 5 and 0.625 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0093] Example 2

[0094] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 5 and 0.833 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0095] Example 3

[0096] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 5 and 1.07 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0097] The specific ratios of the raw materials for preparing the polymer dispersion and the test results of the copper clad laminate with the polymer composite film are shown in Table 2.

[0098] Table 2

[0099]

[0100] The following comparative examples 1-8 synthesize liquid crystal polymer dispersions and polymer dispersions, respectively. After the dispersions are synthesized, the corresponding solutions are coated on a 12 μm copper plate with a thickness of 50 μm, and baked at 350°C to 370°C for 30 min to 60 min, the solvent is removed and heated, and then cooled to form corresponding film materials, thereby obtaining corresponding copper clad laminates, and the mechanical properties and electrical properties of the above copper clad laminates are tested.

[0101] Comparative Example 1

[0102] In a 100 ml reaction bottle, add 3.5 g of LF31-P powder and 31.5 g of NMP in sequence, and stir for 6 hours to allow the powder to be completely dispersed in the solvent to obtain a LF31-P dispersion.

[0103] Comparative Example 2

[0104] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 1 and 0.625 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0105] Comparative Example 3: In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 2 and 0.625 g of LF31-P powder were added in sequence and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0106] Comparative Example 4: In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 3 and 0.625 g of LF31-P powder were added in sequence and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0107] Comparative Example 5

[0108] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 4 and 0.625 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0109] Comparative Example 6

[0110] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 4 and 1.07 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0111] Comparative Example 7

[0112] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 5 and 0.441 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0113] Comparative Example 8

[0114] In a 100 ml reaction bottle, 10 g of the polyamic acid solution synthesized in Synthesis Example 5 and 1.35 g of LF31-P powder were added in sequence, and stirred for 6 hours to allow the powder to be completely dispersed in the polyamic acid solution to obtain a polymer dispersion.

[0115] The specific ratios of the raw materials for preparing the liquid crystal polymer dispersion and the polymer dispersion and the test results of the corresponding copper clad laminate are shown in Table 3.

[0116] Table 3

[0117]

[0118]

[0119] Note: The corresponding test standards in Table 1-3 are: the test standard for peel strength is IPC-TM6502.4.9, the test standard for tin-bleaching test is IPC-TM650 2.4.13, and the test standard for tensile strength and elongation is ASTM D638.

[0120] The LF31-P powder in Table 2-3 was purchased from Nippon Oil & Energy Corporation (JXTG), with an average particle size of <3 μm, and is a fully ester-based crystalline polymer.

[0121] The test results show that: from Comparative Example 1, it can be seen that LF31-P powder (particle size <3μm, fully ester-based crystalline polymer) is dispersed in NMP, but after high-temperature sintering, it cannot form a film by itself.

[0122] It can be seen from Synthesis Examples 1 to 5 that during the synthesis of polyamic acid, a monomer containing a liquid crystal structure (specifically an ester group) is added, so that the copper-clad laminate formed by polyamic acid has an excellent dielectric loss factor Df, and the more liquid crystal structure ratio in the polyamic acid molecular chain, the better the Df value. In Synthesis Example 2, the diamine monomer is APAB, and the dianhydride monomer is TAHQ. Both monomers contain liquid crystal structures, so that the liquid crystal structure content in the molecular chain of polyamic acid is the largest, and Df is lower than the Df value of Synthesis Examples 3 to 5, but the corresponding Dk value increases. At the same time, the peel strength of the composite film on the copper-clad laminate is reduced, and the increase of the liquid crystal structure will reduce the adhesion between the composite film and the copper foil, thereby reducing the peel strength. Synthesis Examples 3 to 5 have flexible structures (specifically -O-) mixed with the same proportion, and the Df value is higher, and the Dk value decreases. At the same time, the addition of the flexible structure improves the adhesion between the composite film and the copper foil, so that the peel strength is improved. The diamine monomer and dianhydride monomer containing a liquid crystal structure added in Synthesis Example 5 are polymerized in a segmented manner, which increases the dispersibility of the liquid crystal structure, thereby obtaining a product having excellent Dk and Df values ​​while maintaining excellent peel strength.

[0123] Examples 1 to 3 use the polyamic acid synthesized in Synthesis Example 5. Compared with Synthesis Example 5, Examples 1 to 3 add LF31-P powder (particle size <3μm) with 20wt% to 30wt% full ester group and insoluble in solvent. The addition of liquid crystal polymer powder can increase the number of crystalline structures, produce a large number of physical crystalline cross-linked structures, and thus improve the mechanical properties of the polymer composite film. The prepared copper clad laminates have excellent Df and Dk, and the dielectric loss factor (Df) and thermal expansion coefficient (CTE) tend to decrease with the increase in the amount of LF31-P powder added. In addition, the peel strength of the polymer composite film reaches the target value (peel strength is greater than or equal to 0.7kgf / cm).

[0124] Compared with Example 1, although the polymer dispersions corresponding to Comparative Examples 3 to 5 are added with the same amount of liquid crystal polymer powder, the addition of liquid crystal polymer powder can increase the number of crystalline structures and produce physical crystalline cross-linked structures, thereby improving the mechanical properties of the polymer composite film, and the Df of the copper clad laminate is also reduced, but the peel strength and thermal expansion coefficient of the polymer composite film are reduced, and the Dk of the copper clad laminate is increased. This is because the diamine monomer and dianhydride monomer used to prepare polyamic acid in Comparative Example 3 are both monomers containing liquid crystal structures, and are not matched with flexible structures, resulting in a decrease in the degree of freedom of the polyamic acid molecules and a decrease in the flexibility of the molecular chain, which makes the compatibility of the polyamic acid molecules with the liquid crystal polymer powder worse, resulting in a decrease in the thermal expansion coefficient and peel strength of the polymer composite film, and an increase in the Dk of the copper clad laminate. In Comparative Examples 4 to 5, the diamine monomer or dianhydride monomer used to prepare polyamic acid is separately introduced into the liquid crystal structure, and the distribution uniformity of the crystalline phase in the network structure is reduced compared with that in Example 1, thereby reducing the number of physical crystallization cross-linking points between the liquid crystal polymer crystalline phase and the polyimide crystalline phase, resulting in a decrease in the Df, peel strength and thermal expansion coefficient of the polymer composite film, while the Dk of the copper clad laminate increases and exceeds the target value (Dk is preferably between 3.2 and 3.3).

[0125] Compared with Example 3, although Comparative Example 6 adds the same amount of liquid crystal polymer powder, which can increase the number of crystalline structures and the physical crystalline cross-linking structure, thereby improving the mechanical properties of the polymer composite film and reducing the Df value of the copper clad laminate, at the same time, the peel strength of the polymer composite film decreases, and the Dk value of the copper clad laminate increases, exceeding the target value.

[0126] The polyamic acid of Synthesis Example 1 used in Comparative Example 2 has no liquid crystal structure, indicating that the polyamic acid without liquid crystal structure has poor compatibility with LF31-P powder, resulting in a decrease in the mechanical properties of the polymer composite film and a significant decrease in the peel strength.

[0127] It can be seen from Examples 1 to 3 and Comparative Examples 7 to 8 that the increase in the amount of LF31-P powder added is conducive to the decrease in the Df value of the copper clad laminate, but the Dk value of the copper clad laminate will increase and the peel strength of the polymer composite film will decrease. In Comparative Example 7, the amount of LF31-P powder added is too little, and the Df value does not reach the target value (Df is preferably between 0.001 and 0.002). In Comparative Example 8, the amount of LF31-P powder added is too much, and the Dk value and peel strength both exceed the target value (Dk is preferably between 3.2 and 3.3).

[0128] In summary, the polymer dispersion provided by the present invention forms a dispersion by mixing a liquid crystal polymer powder with a thermoplastic polyamic acid containing both a liquid crystal structure and a flexible structure, which can effectively improve the solid content and viscosity of the dispersion, and the formed dispersion has good stability, which is conducive to the film formation of the dispersion, and the formed polymer composite film in the copper clad laminate has good adhesion to the copper plate, and at the same time, the two crystal phases formed in the polymer composite film can form a network structure through crystallization cross-linking points, which effectively reduces the Df and thermal expansion coefficient of the copper clad laminate, and at the same time improves the mechanical properties of the polymer composite film.

[0129] The above embodiments and comparative examples are only used to help understand the method of the present invention and its core concept; in addition, for ordinary technicians in this field, various other corresponding changes and modifications can be made based on the technical concept of the present invention, and all these changes and modifications should fall within the scope of protection of the claims of the present invention.

Claims

1. A polymer dispersion, characterized in that: The invention comprises liquid crystal polymer powder, polyamic acid and solvent. The solid components of the polymer dispersion liquid comprise the polyamic acid and the liquid crystal polymer powder. The weight percentage of the liquid crystal polymer powder in the solid components of the polymer dispersion liquid is 20% to 30%, the weight percentage of the polyamic acid in the solid components of the polymer dispersion liquid is 70% to 80%, and the polyamic acid is polymerized by two diamine monomers and two dianhydride monomers. The two diamine monomers and the two dianhydride monomers respectively contain a liquid crystal structure and a flexible structure. The liquid crystal structure contains an ester group, and the flexible structure contains an -O-substituent.

2. The polymer dispersion according to claim 1, characterized in that The particle size of the liquid crystal polymer powder is less than or equal to 3 μm.

3. The polymer dispersion according to claim 1, characterized in that The solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40000cps to 50000cps.

4. The polymer dispersion according to claim 1, characterized in that The liquid crystal polymer powder includes aromatic liquid crystal polyester.

5. A method for preparing a polymer dispersion, characterized in that: The following steps are involved: Providing a polyamic acid solution, the polyamic acid solution comprising polyamic acid and a solvent, the polyamic acid being polymerized by two diamine monomers and two dianhydride monomers, the two diamine monomers and the two dianhydride monomers respectively containing a liquid crystal structure and a flexible structure, the liquid crystal structure containing an ester group, and the flexible structure containing an -O- substituent; and Adding liquid crystal polymer powder to the polyamic acid solution and mixing to obtain the polymer dispersion, The solid component of the polymer dispersion includes the polyamic acid and the liquid crystal polymer powder, the weight percentage of the liquid crystal polymer powder in the solid component of the polymer dispersion is 20% to 30%, and the weight percentage of the polyamic acid in the solid component of the polymer dispersion is 70% to 80%.

6. The method for preparing a polymer dispersion according to claim 5, characterized in that: The average particle size of the liquid crystal polymer powder is less than or equal to 3 μm.

7. The method for preparing a polymer dispersion according to claim 5, characterized in that: The solid content of the polymer dispersion is 25% to 35%, and the viscosity is 40000cps to 50000cps.

8. The method for preparing a polymer dispersion according to claim 5, characterized in that: The liquid crystal polymer powder includes aromatic liquid crystal polyester.

9. The method for preparing a polymer dispersion according to claim 5, characterized in that: The diamine monomer containing a liquid crystal structure includes one or more of p-aminophenyl p-aminobenzoate, 1,4-bis(4-aminophenoxy)benzene and di-p-aminophenyl terephthalate; The diamine monomer containing a flexible structure includes one or more of 4,4'-diaminodiphenyl ether, 2,2'-bis[4-(4-aminophenoxyphenyl)]propane, 1,3-bis(4'-aminophenoxy)benzene and 1,3-bis(3-aminophenoxy)benzene.

10. The method for preparing a polymer dispersion according to claim 5, characterized in that: The dianhydride monomer containing a liquid crystal structure includes 3,3',4,4'-biphenyltetracarboxylic dianhydride, p-phenylene bis(trimellitate) dianhydride and cyclohexane-1,4-diylbis(methylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid ethyl ester); The dianhydride monomer containing a flexible structure includes one or more of 4,4'-oxydiphthalic anhydride and bisphenol A diether dianhydride.

11. A polymer composite membrane, characterized in that: The polymer composite film is prepared by heating the polymer dispersion according to any one of claims 1 to 4, and the polymer composite film includes liquid crystal polymer crystals and polyimide crystals, and the liquid crystal polymer crystals and the polyimide crystals are cross-linked to form a network structure.

12. The polymer composite membrane according to claim 11, characterized in that The weight percentage of the liquid crystal polymer crystals in the polymer composite film is 20% to 30%.

13. The polymer composite membrane according to claim 11, characterized in that: The polymer composite film is anisotropic.

14. A copper clad laminate, characterized in that: It comprises a copper foil and a polymer composite film laminated on at least one surface of the copper foil, wherein the polymer composite film comprises the polymer composite film as claimed in any one of claims 11 to 13.