Anti-coking boron nitride coating technology for aircraft engine fuel nozzle surface

By using plasma-assisted chemical vapor deposition method to grow BN coatings on the surface of the jet engine nozzle, the problem of coking of nozzles and other components is solved, and efficient anti-oxidation coking protection is achieved, which extends the service life and simplifies the process.

CN114657542BActive Publication Date: 2024-11-26HARBIN INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210348132.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-30
Publication Date
2024-11-26
Estimated Expiration
2042-03-30

AI Technical Summary

Technical Problem

Components such as aircraft engine nozzles are prone to coking during fuel delivery, resulting in increased thermal resistance and flow resistance, reducing the nozzle atomization quality and service life. The existing physical coking and chemical decoking methods have problems such as high costs and unstable operation. , it is difficult to effectively prevent coking.

Method used

The BN anti-coking coating is grown on the metal surface of the jet engine nozzle by plasma-assisted chemical vapor deposition method. Through the chemical vapor deposition process, a dense BN coating is generated at high temperatures, reducing the reaction temperature and improving the oxidation resistance and stability of the coating. .

Benefits of technology

Achieves efficient anti-coking protection with uniform coverage on the surface of complex structures, extends the service life of components such as nozzles, reduces the coating preparation temperature and equipment complexity, demonstrates excellent anti-oxidation coking ability, and has a lower thickness that affects mechanical structure. Small.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114657542B_ABST
    Figure CN114657542B_ABST
Patent Text Reader

Abstract

When an aircraft engine is in operation, aviation fuel flows through hot parts, causing the temperature to rise. The fuel is easily oxidized and coked to form carbon deposits under the catalysis of metal on the surface of the engine nozzle, which affects the service life of the aircraft engine and may even cause aviation accidents in severe cases. In addition, the decoking process after the coking is generated also faces the problem of high time and labor costs. The present invention is a coking protective coating technology for metal materials applied to the field of aircraft engine nozzles, specifically a boron nitride anti-coking coating and a chemical vapor deposition preparation method thereof. The boron nitride coating can reduce the catalytic coking effect of metal elements in alloy materials, thereby achieving the purpose of coking inhibition. At the same time, the process has the advantages of simple process, obvious coking inhibition, and easy physical removal of coking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aviation engine hydrocarbon fuel coking inhibition and relates to a process for preparing a BN anti-coking coating by plasma-assisted chemical vapor deposition on the metal surface of an engine nozzle. Background Art

[0002] In the working environment of aircraft engines, during the process of aviation fuel being transported from the fuel tank to the combustion chamber for combustion, it will flow through multiple hot components, such as oil pumps, heat exchangers, and lubricating oil coolers. The fuel will absorb a large amount of heat during transportation, causing the temperature to rise. Studies have shown that when the fuel is heated to a certain temperature, it will undergo a series of reactions such as oxidation, pyrolysis, cracking, dehydrogenation, coking, and polymerization under the catalytic action of oxygen and metals to generate coking and carbon deposits that are eventually deposited on the wall of the component. The generation of coking and carbon deposits will increase the thermal resistance and flow resistance of the nozzle components, reduce the nozzle atomization quality, and reduce the service life of the nozzle and downstream components. In more serious cases, it will directly lead to aviation accidents, posing a serious threat to the flight safety of the aircraft.

[0003] At present, the solutions are divided into physical decoking and chemical decoking. Among them, physical decoking includes returning to the factory for maintenance, gas-liquid purging, etc. This type of process has high operating costs and is easy to affect the engine power and sealing performance, and even cause mid-air parking accidents. Chemical decoking includes two methods: fuel additives and surface modification. Fuel additives often cause fuel component instability and thus interfere with the stable operation of the engine. Surface modification is to process an inert coating on the metal surface to shield the metal catalytic coking effect and reduce the difficulty of coke removal. At present, some of the above methods have been used in the surface protection of aircraft engine nozzles, but coking of the combustion chamber wall and coking blockage of the nozzle still occur. Therefore, the industry is still looking for a process to successfully reduce or eliminate coking and improve the shortcomings of existing technologies.

[0004] BN coating has excellent oxidation resistance, thermal shock resistance, chemical stability and machinability. It has been widely used in the preparation of ceramic-based composite materials for rocket engine combustion chambers, nozzles, aero-engine vector nozzle adjustment plates, liquid rocket gas rudders, missile nose cones, end caps and other components. At the same time, the BN coating prepared by chemical vapor deposition (CVD) has a strong density and can provide good protection for the substrate. Therefore, PECVD can be used to prepare BN coatings and applied to the field of anti-coking of aero-engine nozzles. Summary of the invention

[0005] In view of the current problems in the field of coking inhibition of aircraft engine fuel nozzles, the patent of this invention uses plasma-assisted chemical vapor deposition to directly grow a BN anti-coking coating on the surface of the substrate that needs to be protected from coking. This invention is of great significance for improving the coking inhibition ability of aircraft engine hot parts and improving the stability and service life of hot parts such as engine nozzles.

[0006] To achieve the above objectives, the process scheme adopted by the present invention is: a process for growing a BN anti-coking coating directly on the metal surface of an aircraft engine fuel nozzle by plasma chemical vapor deposition, and the process equipment mainly includes a reaction deposition zone heating device, an atmosphere pressure regulating device, a reaction precursor supply device and a plasma auxiliary device.

[0007] The process for directly growing a BN anti-coking coating on a high-temperature resistant metal surface is characterized in that the specific process for preparing the BN anti-coking coating is as follows: (1) the sample to be coated is subjected to a pretreatment of degreasing and rust removal; (2) the treated sample is placed in a reaction deposition device, the air in the reaction chamber is removed as much as possible through a vacuum system, and a certain flow of carrier gas is introduced through an air inlet; (3) the pressure in the reaction chamber is controlled to a value required by the experiment using the carrier gas flow rate; (4) the heating device is turned on, the temperature and holding time required for the deposition reaction are set, and the reaction deposition zone is heated; (5) the reaction deposition zone is heated to a set temperature, the precursor is heated and evaporated to start the chemical vapor deposition process, and the plasma generator is turned on, and a suitable plasma power is set to assist the reaction; (6) the reaction is terminated after the reaction lasts for a set time, and the temperature is cooled to room temperature at a set cooling rate.

[0008] The chemical vapor deposition process refers to a method of using one or several gaseous compounds or single substances of the elements required for the BN coating as raw materials to carry out chemical reactions on the surface of the sample to generate a thin film. Plasma assistance is to ionize the gas containing the atoms of the film components with the help of microwaves or radio frequencies, thereby enhancing the chemical activity of the plasma, lowering the temperature required for the reaction, and reducing energy consumption. If plasma assistance is not used, atmospheric pressure chemical vapor deposition (APCVD), low pressure chemical vapor deposition (LPCVD), metal organic compound chemical vapor deposition technology (MOCVD) and other methods can also be used, which are also within the scope of protection of this patent application.

[0009] The reaction precursor is a substance that provides the required B and N elements for the preparation of the BN coating. Specifically, it can be a solid borane ammonia complex, a gaseous borazine, or a mixture of one or more gases such as borane, ammonia, nitrogen, diborane, boron trichloride, etc.

[0010] The types of carrier gas include argon, nitrogen, helium, hydrogen or a mixture of several gases; the pressure in the reaction chamber can be selected into different ranges for atmospheric pressure chemical vapor deposition (APCVD) or low pressure chemical vapor deposition (LPCVD) as required.

[0011] The precursor heating temperature needs to be combined with the physical and chemical properties of the precursor itself, in order to ensure that the chemical vapor deposition process occurs on the surface of the sample. Other methods besides heating can also be used, and gaseous precursors can also be used directly to chemically vapor deposit thin films.

[0012] The reaction substrate is a sample protected by a BN anti-coking coating, which may be a hot part of an aero-engine such as an aero-engine nozzle, or may be the surface of other metal samples that require anti-coking protection.

[0013] Compared with the prior art, the advantages of the present invention are:

[0014] The BN coating still exhibits excellent oxidation resistance and chemical stability at 1000°C. At the same time, the 4.2nm thick BN anti-coking coating prepared by the present invention exhibits good anti-oxidation and coking ability. Compared with the composite ceramic coating prepared by other methods, the thickness is lower and the impact on the mechanical structure and thermal conductivity of the original parts is smaller.

[0015] Existing composite material anti-coking coatings or surface strong oxidation treatment methods are difficult to achieve uniform coverage on the surface of complex structural components. The present invention can react on the surface of fine structures through a chemical vapor deposition method to prepare a dense anti-coking coating on the surface of complex structural samples.

[0016] The existing preparation process steps of composite material anti-coking coatings often require multi-step reactions, complex processes, and high equipment requirements. The present invention adopts plasma-assisted chemical vapor deposition, which reduces the coating preparation temperature and prepares the BN anti-coking coating through a one-step chemical vapor deposition reaction, which has a simpler process. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The coking inhibition mechanism and application scenarios of BN coating are shown.

[0018] Figure 2 Optical images and SEM images of the BN coating before and after preparation are shown, demonstrating the dense surface structure of the coating.

[0019] Figure 3 The Raman spectrum of the BN coating is shown, indicating that the BN coating is an hBN structure. The XPS test results show that the bonding mode of B and N in the BN coating is sp 2 In hybridization mode, the ratio of B to N elements is close to 1.05:1.

[0020] Figure 4 The AFM thickness test and TEM test of the BN coating are shown, and the coating thickness increases with the deposition time.

[0021] Figure 5 A schematic diagram of the anti-coking test platform is shown.

[0022] Figure 6 The comparison chart of coking removal effect before and after nitrogen purging of the oxidized coking sample for 6 hours is shown. DETAILED DESCRIPTION

[0023] Taking GH4049 (15×10×0.5mm) plate as the protected part and preparing BN anti-coking coating on the surface as an example, a specific implementation method of directly preparing BN anti-coking coating on the surface of a metal substrate is described. GH4049 is a nickel-based high-temperature alloy, calculated by mass percentage: Cr 9.5-11%, Co 14.0-16.0%, Mo 4.5-5.5%, Ti 1.4-1.9%, the remainder is Ni, trace elements 0.01-0.2%, and trace elements include one or more of C, Al, Mn, P, Fe, B, etc.

[0024] Borane ammonia complex (Sigma Aldrich, 97%) was used as a precursor to grow a BN anti-coking coating on the surface of the component to be protected.

[0025] The borane ammonia complex is a commercial product and is not purified or otherwise treated before use. The single dosage is 50 to 500 mg. The substrate can be a hot component such as an aircraft engine nozzle or a fuel cooler, or a metal or alloy that needs to be protected.

[0026] The surface of the metal sample often has an oxide layer or grease layer left over from the processing or storage process, and the surface is degreased and rusted after alkaline washing, acid washing and neutralization treatment.

[0027] The pretreated metal sample is placed in a tubular furnace, and the air in the tube is removed by a vacuum pump. An argon / hydrogen (Ar:H2=2:1) ​​mixed gas is introduced as the experimental atmosphere, and the system pressure is controlled at 5-30Pa. The heating device is turned on to raise the temperature of the reaction deposition zone to 700-1000°C. At this time, the solid borane ammonia precursor is heated to 90-120°C. The pyrolyzed and gasified borazine reaction molecules are completely decomposed in the plasma generating zone and reach the metal surface to obtain a BN coating through collision dehydrogenation. The deposition time is set to 20-80min. After the experiment is completed, the temperature is lowered, the vacuum pump is turned off, and the mixed gas is continued to be introduced. When the air pressure returns to normal pressure and the temperature drops to room temperature, the sample is taken out.

[0028] Optical photos and scanning electron microscope test images of the BN coating before and after growth in 5 are as follows: Figure 2As shown in the image, it can be clearly seen that the grown BN coating has a dense surface. Figure 3 The Raman spectrum and XPS of the BN coating show that the Raman peak is at 1368 cm -1 Nearby, indicating that the BN coating is hBN structure, BN coating XPS test results show that the B, N bonding mode in the BN coating is sp 2 The hybridization mode, the B:N element ratio is close to 1.05:1, which is close to the element ratio of 1:1, proving that the grown BN coating is hBN structure. Figure 4 The atomic force image shows that the thickness of the BN coating increases with time according to the height of the parabola. Figure 4 Transmission electron microscopy shows that the BN coating thickness is about 10 layers.

[0029] The anti-coking test was completed on an independently designed and constructed anti-coking performance test platform. The platform schematic diagram and equipment diagram are shown in the figure below. Figure 5 The specific components include: fuel supply device, fuel mixture preheating section, coking test tube furnace, exhaust gas treatment section, and Labview analysis platform.

[0030] The anti-coking performance test platform refers to the operating conditions of aircraft engines, and the oxidation coking test conditions can be set in the range of 400-500°C, RP-3 fuel supply rate 40μl / min, fuel preheating temperature 270°C, nitrogen supply rate 150ml / min, and the experimental time is set to 6h.

[0031] The specific steps of the performance test platform are as follows: place the sample to be tested into the center of the furnace temperature of the coking test tube furnace, adjust the gas flowmeter to control the carrier gas flow rate to 150ml / min, and start heating after introducing nitrogen for 20min, and heat it to the coking temperature of 450℃. Turn on the DC power supply to heat the preheating section. The material of the preheating section is selected as a titanium tube, and the current is set at about 3A. Heat the preheating section to 270℃. At this time, inject RP-3 fuel into the preheating section through the fuel microfluidic injector at a rate of 40μl / min. The fuel is heated and vaporized in the tube. In this process, the temperature of the preheating section can be adjusted by observing the gasification of the fuel preheating section outlet to obtain the best gasification effect. The vaporized fuel reaches the furnace temperature center under nitrogen transportation and is oxidized and coked on the sample surface. The experimental time is set to 6h according to demand. Follow-up observations are carried out after the experiment. The SEM test results are as follows Figure 6 As shown, large areas of filamentous coking and partial coking appeared on the unprotected surface, while there was no obvious coking on the surface protected by the BN coating.

[0032] The 9 samples were subjected to a coke removal test, and the sample surface was purged with 10 MPa nitrogen for 5 minutes. It can be seen that the coke removal effect of the samples under BN protection was more obvious, and only part of the lump coke was removed from the unprotected samples.

Claims

1. A process for growing a boron nitride anti-coking coating on the surface of a metal material of an aircraft engine nozzle by plasma-assisted chemical vapor deposition, wherein the process is characterized in that: (1) a sample to be coated is subjected to a pretreatment of degreasing and rust removal; the surface of the metal sample often has an oxide layer or grease layer left over from processing or storage, and the surface is subjected to alkali washing, acid washing and neutralization treatment to degreasing and rust removal; (2) the treated sample is placed in a reaction deposition device, the air in the reaction chamber is removed as much as possible through a vacuum system, and a certain flow of carrier gas is introduced through the air inlet; the carrier gas is a 2:1 mixture of argon and hydrogen ( 3) Using the carrier gas flow rate to control the pressure in the reaction chamber to the value required by the experiment; the pressure is controlled at 5~30Pa (4) Turn on the heating device, set the temperature and holding time required for the deposition reaction, and heat the reaction deposition zone to 700~1000°C; the deposition time is set to 20~80min (5) The reaction deposition zone is heated to the set temperature, the precursor is heated and evaporated to start the chemical vapor deposition process, and the plasma generator is turned on, and the appropriate plasma power is set to assist the reaction; the heating temperature is 90~120°C (6) After the reaction reaches the set time, the reaction is terminated and the temperature is cooled to room temperature at the set cooling rate; The thickness of the boron nitride anti-coking coating is 4.2 nm.

2. The process according to claim 1, characterized in that The reaction precursor is a substance that provides the required B and N elements for the preparation of the BN coating, specifically a mixture of one or more gases selected from borane, ammonia, nitrogen, diborane and boron trichloride, a solid borane-ammine complex or a gaseous borazine.

Citation Information

Cited By

  • Method for analyzing dynamic performance degradation of protective coating-composite sheet in thermal vibration environment

    CN120102619A