Preparation method of back contact battery and back contact battery
By preparing front and back doped source layers on both sides of a silicon substrate and forming different doped layers and front surface field layers through a single diffusion process, the problem of complex and costly fabrication of existing back contact cells is solved, thereby simplifying the process, reducing costs, and improving yield.
Patent Information
- Application Number
- CN202011611876.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-12-30
AI Technical Summary
Existing methods for preparing back-contact batteries are complex and costly, making it difficult to commercialize them.
The process involves fabricating a front-side doped source layer and a back-side doped source layer on both sides of a silicon substrate, and forming different doped layers and a front surface field layer through a single diffusion process, thus simplifying the process flow.
It simplifies the process, reduces production costs, shortens the battery manufacturing cycle, improves yield, and facilitates industrial application.
Smart Images

Figure CN114695594B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cell production, and in particular to a method for preparing a back-contact cell and a back-contact cell. Background Art
[0002] With the rapid development of the photovoltaic industry, domestic and foreign markets have higher and higher requirements for solar cell efficiency and performance, which has also prompted many manufacturers to actively conduct research on new battery structures and production processes in order to gain industry advantages. Interdigitated back contact (IBC) cells refer to solar cells with cross-arranged P and N regions on the back of the cell. They can completely avoid the optical loss caused by the shading of the front electrode grid lines, maximize the use of incident light, and increase short-circuit current. They have received a lot of attention in recent years.
[0003] The surface of existing back-contact batteries usually has three doped regions: a passivation region on the front side of the battery, an emitter region and a back field region on the back side of the battery. For an N-type silicon substrate, the emitter region is a P-type doped layer, and the front passivation region and the back field region are N-type doped layers. The conventional preparation method is to use three diffusions to obtain three different doped layers respectively. The process is relatively complicated, time-consuming, and increases production costs. The industry has disclosed a solution that first diffuses phosphorus on the front side, and then uses phosphorus slurry and boron slurry to co-diffuse to simultaneously obtain the emitter region and back field region on the back side; however, the process of this solution is still relatively complicated, and the performance and process of the boron slurry product are not stable enough at present, and the cost is relatively high, making mass production and promotion more difficult.
[0004] In view of this, it is necessary to provide a new method for preparing a back-contact battery and a back-contact battery. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a back-contact battery and a back-contact battery, which can simplify the process flow, improve the yield rate and reduce the production cost.
[0006] In order to achieve the above-mentioned invention object, the present application provides a method for preparing a back contact battery, which mainly includes:
[0007] Surface treatment of the silicon substrate;
[0008] A front doping source layer and a back doping source layer are prepared on both sides of the silicon substrate, wherein the silicon substrate has a first region corresponding to the back doping source layer and a second region adjacent to the first region;
[0009] Diffusion, so that a front surface field layer is formed on the front side of the silicon substrate, a first doping layer with a doping type consistent with that of the front surface field layer is formed on the back side of the first region, and a second doping layer with a doping type opposite to that of the first doping layer is formed on the back side of the second region;
[0010] Cleaning, coating and metallization are carried out in sequence.
[0011] As a further improvement of the embodiment of the present application, the front doping source layer and the back doping source layer contain the same doping element, and the content of the doping element in the front doping source layer is lower than the content of the doping element in the back doping source layer.
[0012] As a further improvement of the embodiment of the present application, the front doping source layer and the back doping source layer are obtained by screen printing using a predetermined slurry, and the printing thickness of the front doping source layer is smaller than the printing thickness of the back doping source layer; or, the concentration of the doping element in the slurry used for the front doping source layer is smaller than the concentration of the doping element in the slurry used for the back doping source layer.
[0013] As a further improvement of the embodiment of the present application, the thickness of the front doping source layer and the back doping source layer are both set to 0.5-2 μm.
[0014] As a further improvement of the embodiment of the present application, the silicon substrate adopts an N-type silicon wafer, the doping element in the front surface field layer and the first doping layer is phosphorus; and the doping element in the second doping layer is boron.
[0015] As a further improvement of the embodiment of the present application, the phosphorus concentration in the front doping source layer is 0.1% to 5%; the phosphorus concentration in the back doping source layer is 5% to 15%.
[0016] As a further improvement of an embodiment of the present application, the reaction gas used in the diffusion step includes BBr3; the diffusion step includes a first diffusion stage, a second diffusion stage and a third diffusion stage, the temperature of the first diffusion stage is set to 860-1050°C, the temperature of the second diffusion stage is set to 960-1300°C, and the temperature of the third diffusion stage is set to 860-1050°C.
[0017] As a further improvement of the embodiment of the present application, the temperatures of the first diffusion stage, the second diffusion stage and the third diffusion stage are all set between 940 and 980°C.
[0018] As a further improvement of the embodiment of the present application, after the diffusion is completed, a groove is opened on the back side of the silicon substrate so that adjacent first doping layers and second doping layers are spaced apart from each other.
[0019] As a further improvement of the embodiment of the present application, the width of the groove is set to 30-200 μm; the depth of the groove is set to 1-10 μm.
[0020] As a further improvement of an embodiment of the present application, the step of "opening a groove on the back of a silicon substrate" includes preparing a protective layer on the back of the silicon substrate; using a laser window opening method to remove the protective layer at a predetermined position on the back of the silicon substrate; and then performing wet etching to obtain the groove.
[0021] As a further improvement of the embodiment of the present application, the "surface treatment" step includes firstly performing alkaline texturing on both sides of the silicon substrate using an aqueous solution of KOH, NaOH or TMAH; and then polishing the back side of the silicon substrate.
[0022] The present application also provides a back-contact battery manufactured using the aforementioned preparation method.
[0023] The beneficial effects of the present application are: by using the preparation method and back-contact battery of the present application, a back doping source layer and a front doping source layer are first prepared on a partial area on the back side and the front side of the silicon substrate respectively, and then the preparation of the first doping layer, the second doping layer and the front surface field layer can be completed simultaneously through one diffusion, thereby simplifying the process, reducing equipment requirements and production costs, shortening the battery preparation cycle, and improving the battery yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a schematic diagram of the structure of the back contact battery of the present application;
[0025] Figure 2 It is a schematic diagram of the main process of the method for preparing a back contact battery of the present application;
[0026] Figure 3 It is a schematic diagram of the state when the front doping source layer and the back doping source layer are prepared on the surface of the back contact battery of the present application;
[0027] Figure 4 It is a schematic diagram of the state when a protective layer is prepared on the back side of the back contact battery of the present application.
[0028] 100-back contact cell; 1-silicon substrate; 11-first doping layer; 12-second doping layer; 13-groove; 14-front surface field layer; 2-back passivation layer; 3-anti-reflection layer; 41-first electrode; 42-second electrode; 101-front doping source layer; 102-back doping source layer; 103-protective layer. DETAILED DESCRIPTION
[0029] The present invention will be described in detail below in conjunction with the embodiments shown in the accompanying drawings. However, the embodiments do not limit the present invention, and any structural, methodological, or functional changes made by a person skilled in the art based on the embodiments are all within the protection scope of the present invention.
[0030] Ginseng Figure 1As shown, the back-contact battery 100 provided in the present application includes a silicon substrate 1, and a first doping layer 11 and a second doping layer 12 arranged at intervals are formed on the back side of the silicon substrate 1, and the doping types of the first doping layer 11 and the second doping layer 12 are opposite; the back side of the silicon substrate 1 is also recessed to form a groove 13 located between adjacent first doping layers 11 and second doping layers 12 to achieve electrical isolation between the first doping layer 11 and the second doping layer 12.
[0031] In this embodiment, the silicon substrate 1 is an N-type silicon wafer, and the resistivity of the silicon substrate 1 is set to 0.3-7Ω·cm, and the thickness of the silicon wafer is 50-300μm; the first doping layer 11 is an N-type doping layer, and the second doping layer 12 is a P-type doping layer, and the first doping layer 11 and the second doping layer 12 are used as a field passivation region and an emission region, respectively. Generally, the area proportion of the first doping layer 11 is smaller than the area proportion of the second doping layer 12.
[0032] The front surface of the silicon substrate 1 is also formed with a front surface field layer 14, and the front surface field layer 14 is used to improve the front passivation performance. Here, the first doping layer 11 and the front surface field layer 14 are both phosphorus doped layers, and the doping concentration of the front surface field layer 14 is less than the doping concentration of the first doping layer 11. The doping concentration of the first doping layer 11 is preferably 1E21-3E21cm -3 The second doping layer 12 is a boron doping layer, and the doping concentration of the second doping layer 12 is preferably 1E19-3E19cm -3 .
[0033] The thickness of the first doping layer 11 is set to 0.1-1 μm, and the thickness of the second doping layer 12 is set to 0.5-2 μm. The depth of the groove 13 is greater than the thickness of the first doping layer 11 and the second doping layer 12, and the depth of the groove 13 is set to 1-10 μm. The width of the groove 13 is set to 30-200 μm. If the width is too small, it will affect the electrical isolation effect of the adjacent first doping layer 11 and the second doping layer 12, increase the processing difficulty of the groove 13, and make the subsequent film deposition at the position of the groove 13 difficult, and the passivation effect is poor; on the other hand, if the width of the groove 13 is too large, it will affect the area ratio of the emission region and reduce the carrier collection efficiency. For example, the depth of the groove 13 can be set to 2 μm, 5 μm, 8 μm, etc.; the width of the groove 13 is set to 30 μm, 50 μm, 80 μm, 150 μm, etc.
[0034] The back contact cell 100 further includes a back passivation layer 2 disposed on the back side of the silicon substrate 1 , an anti-reflection layer 3 disposed on the front surface field layer 14 , and a metal electrode passing through the back passivation layer 3 and in contact with the silicon substrate 1 .
[0035] The back passivation layer 2 includes at least one of an aluminum oxide film, a silicon oxide film, a silicon nitride film, and a silicon carbide film. The anti-reflection layer 3 can generally be a silicon nitride film, and the film performance and anti-reflection effect of the anti-reflection layer 3 can be improved by adjusting process parameters such as gas flow, reaction time, and temperature. The back passivation layer 2 and the anti-reflection layer 3 can be set as a composite film or a gradient film according to actual product requirements. As an example, the back passivation layer 2 includes an aluminum oxide film and a silicon nitride film stacked on the aluminum oxide film, the thickness of the aluminum oxide film is set to 2 to 10 nm, and the thickness of the silicon nitride film is set to 50 to 100 nm. The metal electrode includes a first electrode 41 in contact with the first doped layer 11 and a second electrode 42 in contact with the second doped layer 12. The first electrode 41 and the second electrode 42 are respectively obtained by screen printing and sintering with a predetermined conductive paste, and the conductive pastes used by the two can be the same or different.
[0036] Combination Figures 2 to 4 As shown, the present application also provides a method for preparing the above-mentioned back contact battery 100, which mainly includes:
[0037] Performing surface treatment on the silicon substrate 1;
[0038] A front doping source layer 101 and a back doping source layer 102 are prepared on both sides of a silicon substrate 1, wherein the silicon substrate 1 has a first region corresponding to the back doping source layer 102 and a second region adjacent to the first region;
[0039] Diffusion, so that a front surface field layer 14 is formed on the front side of the silicon substrate 1, a first doping layer 11 with a doping type consistent with the front surface field layer 14 is formed on the back side of the first region, and a second doping layer 12 with a doping type opposite to the first doping layer 11 is formed on the back side of the second region;
[0040] A groove 13 is formed on the back side of the silicon substrate 1, and the groove 13 is extended along the boundary between the first doping layer 11 and the second doping layer 12, so that adjacent first doping layers 11 and second doping layers 12 are spaced apart from each other;
[0041] Cleaning, coating and metallization are performed in sequence to obtain a back contact cell 100 .
[0042] The "surface treatment" step includes firstly using an aqueous solution of KOH, NaOH or TMAH to perform alkaline texturing on both sides of the silicon substrate 1; and then polishing the back side of the silicon substrate 1. The texturing process can form a pyramid texturing structure of a predetermined height on the surface of the silicon substrate 1 by adjusting the concentration of the solution, the temperature and the reaction time, and can also add a predetermined texturing additive to improve the quality of the texturing according to product requirements; the polishing process is to perform single-sided polishing on the back side of the silicon substrate 1 using an alkaline solution or an acid solution, and the front side of the silicon substrate 1 is usually protected by a water film during the polishing process.
[0043] The front doping source layer 101 and the back doping source layer 102 contain the same doping element. The front doping source layer 101 and the back doping source layer 102 are obtained by screen printing using a predetermined slurry, and the thickness of the front doping source layer 101 and the back doping source layer 102 are both set to 0.5-2 μm.
[0044] In order to make the doping concentration of the front surface field layer 14 lower than the doping concentration of the first doping layer 11, the doping element content in the front doping source layer 101 needs to be lower than the doping element content in the back doping source layer 102. In actual production, the printing thickness of the front doping source layer 102 can be set to be smaller than the printing thickness of the back doping source layer 102; or, different pastes are used to print and form the front doping source layer 101 and the back doping source layer 102 respectively, and the doping element concentration in the paste used in the front doping source layer 101 is lower than the doping element concentration in the paste used in the back doping source layer 102. Here, the phosphorus concentration in the front doping source layer 101 is 0.1% to 5%; the phosphorus concentration in the back doping source layer 102 is 5% to 15%.
[0045] The reaction gas used in the diffusion step includes BBr3; the diffusion step includes a first diffusion stage, a second diffusion stage and a third diffusion stage, the first diffusion stage refers to the stage in which B atoms diffuse into the silicon substrate 1, and the temperature is set to 860-1050°C, the second diffusion stage is the stage of diffusion advancement, so that the above-mentioned B atoms and the P atoms in the front doping source layer 101 and the back doping source layer 102 are advanced into the silicon substrate 1 to increase the junction depth, and the temperature is set to 960-1300°C; the third diffusion stage is mainly to oxidize the back side of the second region of the silicon substrate 1, that is, the B-rich region to form BSG, reduce surface recombination, and also oxidize the residual phosphorus slurry through O2, which is beneficial to subsequent cleaning, and the temperature of this stage is set to 860-1050°C. Preferably, the temperatures of the first diffusion stage, the second diffusion stage and the third diffusion stage are all set between 940-980°C.
[0046] After the diffusion is completed, the surface of the silicon substrate 1 needs to be cleaned to remove the residual phosphorus-containing slurry; and then the groove 13 is prepared. The step of "opening a groove 13 on the back of the silicon substrate 1" includes preparing a protective layer 103 on the back of the silicon substrate 1; using a laser window opening method to remove the protective layer 103 at a predetermined position on the back of the silicon substrate 1; and then performing wet etching to obtain the groove 13. Among them, the protective layer 103 can specifically be a silicon oxide film, and its thickness can be set at 10 to 200μm; the laser wavelength used for the laser window opening is set to 280 to 1000nm, and specifically a laser beam with a wavelength of 355nm, 515nm, 532nm, etc. can be used for the aforementioned laser window opening.
[0047] After the silicon substrate 1 is cleaned and dried, it is plated. The aluminum oxide film can be deposited by ALD or PECVD; the silicon nitride film is prepared by PECVD. The metallization step refers to obtaining a predetermined electrode pattern on the back passivation layer 2 by screen printing, and obtaining a corresponding metal electrode by high-temperature sintering. Here, the first electrode 41 and the second electrode 42 can use silver paste of the same specification to facilitate production and preparation; they can also be printed separately using different conductive pastes according to product requirements, and then sintered.
[0048] Of course, the preparation method may also include steps such as testing, grading and anti-attenuation treatment of the back contact battery 100 that has completed the metallization process, which will not be described in detail here.
[0049] To sum up, the preparation method of the back contact battery 100 of the present application can simultaneously complete the preparation of the first doping layer 11, the second doping layer 12 and the front surface field layer 14 through the preparation of the front doping source layer 101 and the back doping source layer 102 through one diffusion, thereby simplifying the process, reducing equipment requirements and production costs, shortening the battery preparation cycle, and improving the battery yield, which is conducive to industrial promotion and application.
[0050] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0051] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a back contact battery, Features: Surface treatment of the silicon substrate; A front doping source layer and a back doping source layer are prepared on both sides of the silicon substrate, wherein the front doping source layer and the back doping source layer are obtained by screen printing using a predetermined slurry, and the silicon substrate has a first region corresponding to the back doping source layer and a second region adjacent to the first region; Diffusion is performed so that a front surface field layer is formed on the front side of the silicon substrate, a first doping layer with a doping type consistent with that of the front surface field layer is formed on the back side of the first region, and a second doping layer with a doping type opposite to that of the first doping layer is formed on the back side of the second region, wherein the doping elements in the front surface field layer and the first doping layer are phosphorus; and the doping element in the second doping layer is boron; and the reaction gas used in the diffusion step includes BBr 3 ; Cleaning, coating and metallization are carried out in sequence; Among them, the diffusion step includes a first diffusion stage, a second diffusion stage, and a third diffusion stage. In the first diffusion stage, B atoms diffuse into the silicon substrate, and the temperature is set to 860-1050°C; in the second diffusion stage, B atoms and P atoms in the front doping source layer and the back doping source layer are pushed into the interior of the silicon substrate, and the temperature is set to 960-1300°C. In the third diffusion stage, BSG is oxidized on the back side of the second region of the silicon substrate, and the temperature is set to 860-1050°C.
2. The preparation method according to claim 1, Features: The front doping source layer and the back doping source layer contain the same doping element, and the content of the doping element in the front doping source layer is lower than the content of the doping element in the back doping source layer.
3. The preparation method according to claim 2, Features: The printing thickness of the front doping source layer is smaller than the printing thickness of the back doping source layer; or, the concentration of the doping element in the slurry used for the front doping source layer is smaller than the concentration of the doping element in the slurry used for the back doping source layer.
4. The preparation method according to any one of claims 1 to 3, Features: The thickness of the front doping source layer and the back doping source layer are both set to 0.5-2 μm.
5. The preparation method according to claim 1, Features: The silicon substrate is an N-type silicon wafer.
6. The preparation method according to claim 5, Features: The phosphorus concentration in the front doping source layer is 0.1% to 5%; the phosphorus concentration in the back doping source layer is 5% to 15%.
7. The preparation method according to claim 1, Features: The temperatures of the first diffusion stage, the second diffusion stage and the third diffusion stage are all set between 940 and 980°C.
8. The preparation method according to claim 1, Features: After the diffusion is completed, a groove is opened on the back side of the silicon substrate so that the adjacent first doping layers and second doping layers are spaced apart from each other.
9. The preparation method according to claim 8, Features: The width of the groove is set to be 30-200 μm; the depth of the groove is set to be 1-10 μm.
10. The preparation method according to claim 8, Features: The step of "forming a groove on the back side of the silicon substrate" includes preparing a protective layer on the back side of the silicon substrate; removing the protective layer at a predetermined position on the back side of the silicon substrate by a laser window opening method; and then performing wet etching to obtain the groove.
11. The preparation method according to claim 1, Features: The "surface treatment" step includes firstly performing alkaline texturing on both sides of the silicon substrate using an aqueous solution of KOH, NaOH or TMAH; and then polishing the back side of the silicon substrate.
12. A back contact battery, Features: The back contact cell is prepared by the preparation method according to any one of claims 1 to 11.
Citation Information
Patent Citations
Back contact photovoltaic solar cells with grooves
CN102246324A
Method for manufacturing back contact solar cell
CN103794679A
A finger cross back contact solar cell with an isolation region and a preparation method thereof
CN108987503A
Back junction and back contact solar cell and manufacturing method thereof
CN112133793A
Back contact battery and preparation method thereof
CN114765224A