Light-emitting diode epitaxial wafer with improved n-type layer and preparation method thereof
By adopting a specific n-type layer structure in the light-emitting diode epitaxial wafer, including multi-layer gallium nitride sub-layers and silicon-doped gallium nitride sub-layers, the problems of insufficient quality of the n-type GaN layer and electron backflow are solved, and the quality of the light-emitting diode is improved. luminous efficiency and stability.
Patent Information
- Application Number
- CN202210204171.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-03
AI Technical Summary
The quality of the n-type GaN layer in existing light-emitting diode epitaxial wafers is insufficient, resulting in serious electron backflow, which reduces the internal quantum efficiency and light extraction efficiency of the material.
Using an n-type layer structure including a first aluminum gallium nitride sub-layer, a first gallium nitride sub-layer, a first silicon-doped gallium nitride sub-layer and a second silicon-doped gallium nitride sub-layer, by adjusting the doping concentration and The layer thickness ratio blocks the backflow of electrons and improves the recombination luminous efficiency of electrons.
It effectively improves the quality of the n-type layer and the luminous efficiency of the light-emitting diode epitaxial wafer, reduces electron backflow, enhances the stability and active area of electrons, and improves the overall luminous performance.
Smart Images

Figure CN114725255B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of light emitting diode manufacturing, and in particular to a light emitting diode epitaxial wafer with an improved n-type layer and a manufacturing method thereof. Background Art
[0002] Light-emitting diodes are semiconductor electronic components that can emit light. As a new type of efficient, environmentally friendly, green solid-state lighting source, they are rapidly and widely used, such as traffic lights, car interior and exterior lights, urban landscape lighting, mobile phone backlights, etc. Improving the chip's luminous efficiency is the goal that light-emitting diodes are constantly pursuing.
[0003] The light-emitting diode epitaxial wafer is the basic structure for preparing light-emitting diodes. The light-emitting diode epitaxial wafer includes at least a substrate and an undoped GaN layer, an n-type layer, a light-emitting layer and a p-type layer on the substrate. The electrons provided by the n-type layer and the holes provided by the p-type layer enter the light-emitting layer to recombine and emit light.
[0004] The n-type layer is usually an n-type GaN layer, which needs to provide a large number of electrons. Therefore, a large number of Si impurities need to be added to the n-type GaN layer, resulting in the final n-type GaN layer having poor quality. In addition, during the working process after the electric field is actually applied to the epitaxial wafer, there will be a phenomenon that electrons flow back from the light-emitting layer to the n-type GaN layer, and cannot effectively reach the active area to radiate and recombine with holes, which reduces the internal quantum efficiency of the material and affects the light extraction efficiency of the epitaxial wafer itself. Summary of the invention
[0005] The embodiments of the present disclosure provide a light-emitting diode epitaxial wafer with an improved n-type layer and a method for preparing the same, which can improve the quality of the n-type layer, reduce the reflux of electrons, and thus improve the luminous efficiency of the light-emitting diode epitaxial wafer. The technical solution is as follows:
[0006] The embodiment of the present disclosure provides a light emitting diode epitaxial wafer with an improved n-type layer, the light emitting diode epitaxial wafer with an improved n-type layer comprises a substrate and a non-doped GaN layer, an n-type layer, a light emitting layer and a p-type layer sequentially stacked on the substrate.
[0007] The n-type layer includes a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer stacked in sequence, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
[0008] Optionally, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is 0.9-1.5 10 19 cm -3The doping concentration of silicon in the second silicon-doped gallium nitride sublayer is 1.5 to 4 10 19 cm -3 .
[0009] Optionally, the thickness of the first aluminum gallium nitride sublayer is smaller than the thickness of the second aluminum gallium nitride sublayer, and the thickness of the first silicon-doped gallium nitride sublayer is smaller than the thickness of the second silicon-doped gallium nitride sublayer.
[0010] Optionally, the ratio of the thickness of the first aluminum gallium nitride sublayer to the thickness of the second aluminum gallium nitride sublayer is 1:8-1:15, and the ratio of the thickness of the first silicon-doped gallium nitride sublayer to the thickness of the second silicon-doped gallium nitride sublayer is 1:100-1:120.
[0011] Optionally, the thickness of the first gallium nitride sublayer is 18 nm to 300 nm.
[0012] Optionally, the second aluminum gallium nitride sublayer is doped with silicon, and the doping concentration of silicon in the second aluminum gallium nitride sublayer is lower than the doping concentration of silicon in the first gallium nitride sublayer.
[0013] Optionally, the doping concentration of silicon in the second aluminum gallium nitride sublayer is 1.5*10 19 cm -3 ~4*10 19 cm -3 .
[0014] The embodiment of the present disclosure provides a method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer, the method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer comprising:
[0015] providing a substrate;
[0016] An undoped GaN layer, an n-type layer, a light-emitting layer and a p-type layer are sequentially grown on the substrate, the n-type layer comprises a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer which are sequentially stacked, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
[0017] Optionally, the n-type layer is grown in an atmosphere of a mixture of hydrogen, ammonia and nitrogen, the volume ratio of hydrogen to ammonia in the atmosphere for the growth of the first silicon-doped gallium nitride sublayer is 2:1, and the volume ratio of hydrogen to ammonia in the atmosphere for the growth of the first aluminum gallium nitride sublayer, the first silicon-doped gallium nitride sublayer, the second silicon-doped gallium nitride sublayer and the second aluminum gallium nitride sublayer are all 3:2.
[0018] Optionally, the percentage of nitrogen in the atmosphere in which the first silicon-doped gallium nitride sublayer grows is 15%.
[0019] The technical solution provided by the embodiments of the present disclosure has the following beneficial effects:
[0020] The n-type layer is configured to include a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer stacked in sequence. The first aluminum gallium nitride sublayer can block the electrons in the first silicon-doped gallium nitride sublayer and the second silicon-doped gallium nitride sublayer from flowing back to the non-doped GaN sublayer, so that more electrons can enter the light-emitting layer for composite light emission. The first gallium nitride sublayer can play a transitional role, improve the quality of the gallium nitride material that needs to be doped with silicon grown on the first aluminum gallium nitride sublayer, so that the overall quality of the first silicon-doped gallium nitride sublayer and the second silicon-doped gallium nitride sublayer grown on the first gallium nitride sublayer is better, ensuring the overall quality of the n-type layer and the stable supply of electrons. The doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, which can ensure the quality of the second silicon-doped gallium nitride sublayer and facilitate the movement of electrons from the n-type layer to the light-emitting layer. The second aluminum gallium nitride sublayer stacked on the second silicon-doped gallium nitride sublayer can block the electrons from flowing back from the light-emitting layer to the n-type layer, ensuring the stable light emission of the electrons. The Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer. The first aluminum gallium nitride sublayer can effectively isolate the electrons, ensuring that the active area of the electrons is mainly located in the n-type layer and the light-emitting layer. The potential barrier of the second aluminum gallium nitride is relatively low, which can reduce the possibility of electron backflow. At the same time, when the electron concentration in the second silicon-doped gallium nitride layer close to the second aluminum gallium nitride sublayer is high and an electric field is applied, it can ensure that the electrons stably enter the light-emitting layer from the n-type layer for composite light emission. The quality of the n-type layer can be improved and the light-emitting efficiency of the light-emitting diode epitaxial wafer can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 It is a schematic structural diagram of a light-emitting diode epitaxial wafer with an improved n-type layer provided by an embodiment of the present disclosure;
[0023] Figure 2 It is a flow chart of a method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer provided by an embodiment of the present disclosure;
[0024] Figure 3 It is a schematic structural diagram of another light-emitting diode epitaxial wafer with improved n-type layer provided by an embodiment of the present disclosure;
[0025] Figure 4 It is a flow chart of another method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0026] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0027] Figure 1 is a schematic diagram of the structure of a light emitting diode epitaxial wafer with an improved n-type layer provided by an embodiment of the present disclosure, with reference to Figure 1 It can be seen that the embodiment of the present disclosure provides a light-emitting diode epitaxial wafer with an improved n-type layer, which includes a substrate 1 and an undoped GaN layer 2, an n-type layer 3, a light-emitting layer 4 and a p-type layer 5 stacked in sequence on the substrate 1.
[0028] The n-type layer 3 includes a first aluminum gallium nitride sublayer 31, a first gallium nitride sublayer 32, a first silicon-doped gallium nitride sublayer 33, a second silicon-doped gallium nitride sublayer 34 and a second aluminum gallium nitride sublayer 35 which are stacked in sequence. The doping concentration of silicon in the first silicon-doped gallium nitride sublayer 33 is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer 34, and the Al component in the first aluminum gallium nitride sublayer 31 is higher than the Al component in the second aluminum gallium nitride sublayer 35.
[0029] The n-type layer 3 is configured to include a first aluminum gallium nitride sublayer 31, a first gallium nitride sublayer 32, a first silicon-doped gallium nitride sublayer 33, a second silicon-doped gallium nitride sublayer 34 and a second aluminum gallium nitride sublayer 35 stacked in sequence. The first aluminum gallium nitride sublayer 31 can block the electrons in the first silicon-doped gallium nitride sublayer 33 and the second silicon-doped gallium nitride sublayer 34 from flowing back to the non-doped GaN sublayer, so that more electrons can enter the light-emitting layer 4 for composite light emission. The first gallium nitride sublayer 32 can play a transitional role, improve the quality of the gallium nitride material that needs to be doped with silicon grown on the first aluminum gallium nitride sublayer 31, so that the first silicon-doped gallium nitride sublayer 33 and the second silicon-doped gallium nitride sublayer 34 grown on the first gallium nitride sublayer 32 have better overall quality, ensuring the overall quality of the n-type layer 3 and the stable supply of electrons. The doping concentration of silicon in the first silicon-doped gallium nitride sublayer 33 is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer 34, which can ensure the quality of the second silicon-doped gallium nitride sublayer 34 and facilitate the movement of electrons from the n-type layer 3 to the light-emitting layer 4. The second aluminum gallium nitride sublayer 35 stacked on the second silicon-doped gallium nitride sublayer 34 can block the electrons from flowing back from the light-emitting layer 4 to the n-type layer 3, ensuring the stable light emission of the electrons. In addition, the Al component in the first aluminum gallium nitride sublayer 31 is higher than the Al component in the second aluminum gallium nitride sublayer 35. The first aluminum gallium nitride sublayer 31 can effectively isolate the electrons, ensuring that the active area of the electrons is mainly located in the n-type layer 3 and the light-emitting layer 4. The potential barrier of the second aluminum gallium nitride is relatively low, which can reduce the possibility of electron backflow. At the same time, when the electron concentration in the second silicon-doped gallium nitride layer close to the second aluminum gallium nitride sublayer 35 is high and an electric field is applied, it can ensure that the electrons stably enter the light-emitting layer 4 from the n-type layer 3 for composite light emission. The quality of the n-type layer 3 can be improved and the light-emitting efficiency of the light-emitting diode epitaxial wafer can be improved.
[0030] Optionally, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer 33 is 0.9-1.5 10 19 cm -3 The doping concentration of silicon in the second silicon-doped gallium nitride sublayer 34 is 1.5 to 4 10 19 cm -3 .
[0031] When the doping concentrations of silicon in the first silicon-doped gallium nitride sublayer 33 and the second silicon-doped gallium nitride sublayer 34 are respectively within the above ranges, it can be ensured that the quality of the first silicon-doped gallium nitride sublayer 33 and the second silicon-doped gallium nitride sublayer 34 is good, and sufficient electrons can be provided as a whole to ensure that the luminous efficiency of the finally obtained light-emitting diode epitaxial wafer is high.
[0032] For example, the Al content in the first aluminum gallium nitride sublayer 31 may be 0.5-0.8, and the Al content in the second aluminum gallium nitride sublayer 35 may be 0.2-0.4.
[0033] The Al components in the first aluminum gallium nitride sublayer 31 and the second aluminum gallium nitride sublayer 35 are respectively within the above ranges, which can ensure that the first aluminum gallium nitride sublayer 31 and the second aluminum gallium nitride sublayer 35 themselves have good quality, and can also effectively block the backflow of electrons, and promote more electrons to recombine and emit light in the light-emitting layer 4, so as to improve the luminous efficiency of the final light-emitting diode epitaxial wafer.
[0034] For example, the thickness of the n-type layer 3 may be 2 to 9 micrometers, which can ensure that the n-type layer 3 can provide sufficient electrons while ensuring the quality of the obtained n-type layer 3.
[0035] Optionally, the thickness of the first aluminum gallium nitride sublayer 31 is smaller than the thickness of the second aluminum gallium nitride sublayer 35 , and the thickness of the first silicon-doped gallium nitride sublayer 33 is smaller than the thickness of the second silicon-doped gallium nitride sublayer 34 .
[0036] The thickness of the first aluminum gallium nitride sublayer 31 is less than the thickness of the second aluminum gallium nitride sublayer 35, which can ensure that the first aluminum gallium nitride sublayer 31 can achieve good blocking of the electrons as a whole, effectively reduce the possibility that electrons may enter the non-doped GaN layer 2 from the n-type layer 3, and increase the electron concentration in the n-type layer 3 and the light-emitting layer 4. At the same time, the thickness of the second aluminum gallium nitride sublayer 35 is also relatively reasonable, which can block the backflow of electrons and will not excessively increase the overall preparation cost of the light-emitting diode epitaxial wafer. The thickness of the first silicon-doped gallium nitride sublayer 33 is less than the thickness of the second silicon-doped gallium nitride sublayer 34. The first silicon-doped gallium nitride sublayer 33 itself can play a role in transition and provide a part of the electrons, and can also reduce the probability of electrons flowing from the light-emitting layer 4 to the n-type layer 3. Finally, the second silicon-doped gallium nitride sublayer 34 with a larger thickness can achieve stable and large-scale supply of electrons. The overall can effectively reduce the backflow of electrons while ensuring sufficient supply of electrons.
[0037] Optionally, the thickness ratio of the first aluminum gallium nitride sublayer 31 to the second aluminum gallium nitride sublayer 35 is 1:8-1:15, and the thickness ratio of the first silicon-doped gallium nitride sublayer 33 to the second silicon-doped gallium nitride sublayer 34 is 1:100-1:120.
[0038] When the thickness ratio of the first aluminum gallium nitride sublayer 31 to the second aluminum gallium nitride sublayer 35 and the thickness ratio of the first silicon-doped gallium nitride sublayer 33 to the second silicon-doped gallium nitride sublayer 34 are respectively within the above ranges, the light-emitting efficiency of the obtained light-emitting diode epitaxial wafer is relatively high. The overall preparation cost of the light-emitting diode epitaxial wafer is also relatively reasonable and will not be too high, resulting in an excessive increase in the overall preparation cost of the light-emitting diode epitaxial wafer.
[0039] Optionally, the thickness of the first gallium nitride sublayer 32 is 18 nm to 300 nm.
[0040] The thickness of the first gallium nitride sublayer 32 is within the above range, which can meet the transition requirements of n-type layers 3 with different thickness specifications, and the quality of the obtained n-type layers 3 is good.
[0041] For example, the thickness of the first aluminum gallium nitride sublayer 31, the thickness of the first silicon-doped gallium nitride sublayer 33, the thickness of the second silicon-doped gallium nitride sublayer 34 and the thickness of the second aluminum gallium nitride sublayer 35 may be 0.3 μm to 0.6 μm, 0.3 μm to 1.8 μm, 1.8 μm to 5.5 μm and 2.4 μm to 4.5 μm, respectively.
[0042] When the thickness of the first aluminum gallium nitride sublayer 31, the thickness of the first silicon-doped gallium nitride sublayer 33, the thickness of the second silicon-doped gallium nitride sublayer 34, and the thickness of the second aluminum gallium nitride sublayer 35 are respectively within the above ranges, a light-emitting diode epitaxial wafer with better quality and more reasonable cost can be obtained, and the luminous efficiency of the light-emitting diode epitaxial wafer itself can also be greatly improved.
[0043] Optionally, the second aluminum gallium nitride sublayer 35 is doped with silicon, and the doping concentration of silicon in the second aluminum gallium nitride sublayer 35 is lower than the doping concentration of silicon in the first gallium nitride sublayer 32 .
[0044] The second aluminum gallium nitride sublayer 35 is also doped with silicon, which can ensure that the second aluminum gallium nitride sublayer 35 can also provide a part of electrons to offset the effect of the second aluminum gallium nitride sublayer 35 itself blocking electrons, ensuring the stable supply of electrons in the light-emitting layer, while the electrons entering the light-emitting layer 4 from the n-type layer 3 will still be blocked by the second aluminum gallium nitride sublayer 35. In addition, the doping concentration of silicon in the second aluminum gallium nitride sublayer 35 is low, which can ensure the quality of the second aluminum gallium nitride sublayer 35 and the crystal quality of the light-emitting layer 4 grown on the second aluminum gallium nitride sublayer 35. The luminous efficiency of the light-emitting layer 4 is guaranteed.
[0045] Optionally, the doping concentration of silicon in the second aluminum gallium nitride sublayer 35 is 1.5*10 19 cm -3 ~4*10 19 cm -3 .
[0046] The doping concentration of silicon in the second aluminum gallium nitride sublayer 35 is within the above range, the second aluminum gallium nitride sublayer 35 itself has good quality, and can ensure that electrons stably enter the light-emitting layer 4 .
[0047] Figure 2 is a flow chart of a method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer provided by an embodiment of the present disclosure. Figure 2 The method for preparing a light emitting diode epitaxial wafer with an improved n-type layer is used to prepare Figure 1 The light emitting diode epitaxial wafer with improved n-type layer shown in FIG. Figure 2 It can be seen that the embodiment of the present disclosure provides a method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer, and the method for preparing a light-emitting diode epitaxial wafer with an improved n-type layer includes:
[0048] S101: providing a substrate;
[0049] S102: growing an undoped GaN layer, an n-type layer, a light-emitting layer and a p-type layer in sequence on the substrate, wherein the n-type layer comprises a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer stacked in sequence, wherein the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
[0050] Figure 2 The technical effect of the preparation method of the light-emitting diode epitaxial wafer shown in can be referred to Figure 1 The technical effect corresponding to the structure of the light-emitting diode epitaxial wafer shown in FIG. 1 is not described in detail here.
[0051] It should be noted that the first gallium nitride sub-layer is prepared using intrinsic materials.
[0052] Optionally, in step S102 , the growth temperature and growth pressure of the n-type layer may be in the range of 1000-1200° C., respectively, which can ensure that the quality of the obtained n-type layer is good.
[0053] Exemplarily, the n-type layer is grown in an atmosphere of a mixture of hydrogen, ammonia and nitrogen, the volume ratio of hydrogen to ammonia in the atmosphere in which the first silicon-doped gallium nitride sublayer is grown is 2:1, and the volume ratio of hydrogen to ammonia in the atmosphere in which the first aluminum gallium nitride sublayer, the first silicon-doped gallium nitride sublayer, the second silicon-doped gallium nitride sublayer and the second aluminum gallium nitride sublayer are all 3:2.
[0054] The n-type layer is grown in an atmosphere of hydrogen, ammonia and nitrogen, which can reasonably control the growth quality and growth rate of the n-type layer, and effectively ensure the growth efficiency of the n-type layer while ensuring the growth quality of the n-type layer. The volume ratio of hydrogen to ammonia in the atmosphere of the growth of the first silicon-doped gallium nitride sublayer is 2:1, and the volume ratio of hydrogen to ammonia in the atmosphere of the growth of the first aluminum gallium nitride sublayer, the first silicon-doped gallium nitride sublayer, the second silicon-doped gallium nitride sublayer and the second aluminum gallium nitride sublayer is 3:2, which can ensure that when the first silicon-doped gallium nitride sublayer grows, there is more hydrogen in the reaction chamber, and hydrogen has a certain etching tendency, which can form certain etching-like pits on the surface of the first silicon-doped gallium nitride sublayer, and these pits can release stress, reduce the stress in the first silicon-doped gallium nitride sublayer and the strain and dislocation caused by the stress, and improve the quality of the second silicon-doped gallium nitride sublayer grown on the first silicon-doped gallium nitride sublayer to improve the overall crystal quality of the n-type layer.
[0055] It should be noted that the atmosphere environment refers to the atmosphere environment in the reaction chamber of the MOCVD device when a specific epitaxial material is grown in the MOCVD device.
[0056] Optionally, the percentage of nitrogen in the atmosphere for growing the first silicon-doped gallium nitride sub-layer is 15%.
[0057] The percentage of nitrogen in the atmosphere of the growth of the first silicon-doped gallium nitride sublayer is 15%, and the nitrogen can promote the flow of gas in the reaction chamber to improve the growth efficiency of the first silicon-doped gallium nitride sublayer. It can promote the formation of the first silicon-doped gallium nitride sublayer, and with the certain etching effect of hydrogen, it can ensure the rapid growth of the first silicon-doped gallium nitride sublayer, and can play an effective role in releasing stress as a whole.
[0058] In an implementation provided by the present disclosure, the growth temperature of the first aluminum gallium nitride sublayer may be 1000° C., the growth pressure of the first aluminum gallium nitride sublayer may be 100 Torr, the growth speed of the first aluminum gallium nitride sublayer may be 750 rpm, and the atmosphere during the growth of the first aluminum gallium nitride sublayer may be H 2 :NH 3 The atmosphere is about 3:2, accounting for 90% of the total gas volume, and the rest is N 2 Supplement; The growth temperatures of the first gallium nitride sublayer and the second silicon-doped gallium nitride sublayer are 1120°C and 1110°C respectively, the growth pressure and growth speed of the first gallium nitride sublayer and the second silicon-doped gallium nitride sublayer are both 150 Torr and 650 rpm, and the first gallium nitride sublayer and the second silicon-doped gallium nitride sublayer are grown in an atmosphere of H 2 :NH 3 The atmosphere is about 3:2, accounting for 90% of the total gas volume, and the rest is N 2Supplement; the growth temperature of the first silicon-doped gallium nitride sublayer is 1050°C, the growth pressure of the first silicon-doped gallium nitride sublayer is 150Torr, the growth speed of the first silicon-doped gallium nitride sublayer is 600rpm, and the first silicon-doped gallium nitride sublayer is in the atmosphere during growth, H 2 :NH 3 The atmosphere ratio is about 2:1, accounting for 85% of the total gas volume, and the rest is N 2 Supplement; the growth temperature of the second aluminum gallium nitride sublayer is 1000°C, the growth pressure of the second aluminum gallium nitride sublayer is 100Torr, the growth speed of the second aluminum gallium nitride sublayer is 850rpm, and the second aluminum gallium nitride sublayer is in the atmosphere during growth, H 2 :NH 3 The atmosphere is about 3:2, accounting for 90% of the total gas volume, and the rest is N 2 As a whole, a good quality n-type layer can be obtained.
[0059] Figure 3 is a schematic diagram of the structure of another light emitting diode epitaxial wafer with improved n-type layer provided by the embodiment of the present disclosure, with reference to Figure 3 It can be known that in another implementation provided by the present disclosure, the light emitting diode epitaxial wafer may include a substrate 1 and a buffer layer 6, an n-type layer 3, a light emitting layer 4, an AlGaN electron blocking layer 7, a p-type layer 5 and a p-type contact layer 8 grown on the substrate 1. The n-type layer 3 includes a first aluminum gallium nitride sublayer 31, a first gallium nitride sublayer 32, a first silicon-doped gallium nitride sublayer 33, a second silicon-doped gallium nitride sublayer 34 and a second aluminum gallium nitride sublayer 35 stacked in sequence, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer 33 is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer 34, and the Al component in the first aluminum gallium nitride sublayer 31 is higher than the Al component in the second aluminum gallium nitride sublayer 35.
[0060] It should be noted that Figure 3 The n-type layer 3 shown in FIG. Figure 1 The structure of the n-type layer 3 shown in FIG. 1 is the same as that of the n-type layer 3 shown in FIG. 1 , and thus will not be described in detail here.
[0061] Optionally, the substrate 1 may be a sapphire substrate 1. It is easy to manufacture and obtain.
[0062] For example, the buffer layer 6 may include a GaN buffer layer 6 sequentially stacked on the substrate 1, which can effectively alleviate the lattice mismatch.
[0063] In other implementations provided by the present disclosure, the buffer layer 6 may also be one of aluminum nitride, aluminum gallium nitride, or aluminum indium gallium nitride, which is not limited by the present disclosure.
[0064] Exemplarily, the light emitting layer 4 includes a plurality of alternately stacked InGaN well layers and GaN barrier layers. The thickness of the InGaN well layer may be 2 to 5 nm, and the thickness of the GaN barrier layer may be 8 to 20 nm.
[0065] For example, the overall thickness of the light-emitting layer 4 may be 50 to 130 nm, and the molar content of In may be 13% to 25%.
[0066] Optionally, the Al composition in the AlGaN electron blocking layer 7 may be 0.15-0.25, which has a better effect of blocking electrons.
[0067] Optionally, the thickness of the AlGaN electron blocking layer 7 may be 20-100 nm. The obtained AlGaN electron blocking layer 7 has good quality.
[0068] It can provide sufficient holes and ensure that the overall cost of the light-emitting diode epitaxial wafer is not too high.
[0069] Optionally, the p-type layer 5 may be a p-type GaN layer, which is easy to realize and obtain.
[0070] By way of example, the thickness of the p-type contact layer 8 may be 10 to 50 nm.
[0071] It should be noted that in other implementations provided in the present disclosure, the light-emitting diode epitaxial wafer may also include other hierarchical structures, and the present disclosure does not limit this.
[0072] Figure 4 is another flow chart of a method for preparing a light emitting diode epitaxial wafer with an improved n-type layer provided by an embodiment of the present disclosure, refer to Figure 4 It can be seen that the method for preparing a light-emitting diode epitaxial wafer provided in the present disclosure may include:
[0073] S201: providing a substrate.
[0074] The substrate may be a sapphire substrate, which is easy to implement and manufacture.
[0075] Optionally, step S201 may further include: processing the substrate surface for 6 to 10 minutes in a hydrogen atmosphere.
[0076] For example, when processing the substrate surface, the temperature of the reaction chamber may be 1000-1200° C., and the pressure of the reaction chamber may be 200-500 Torr.
[0077] In an implementation provided by the present disclosure, when processing a substrate, the temperature of the reaction chamber may also be 1100° C., and the time for processing the surface of the substrate may be 8 minutes.
[0078] Step S201 may also include: performing nitridation treatment on the surface of the substrate to lay a layer of nitrogen atoms on the surface of the substrate, which can facilitate the rapid growth of gallium nitride materials.
[0079] S202: growing a buffer layer on a substrate.
[0080] Optionally, the temperature of the reaction chamber is controlled to be 450° C. to 600° C., and the pressure of the reaction chamber is controlled to be 200 torr to 500 torr to grow the GaN buffer layer, thereby obtaining a buffer layer of good quality.
[0081] S203: growing a non-doped GaN layer on the buffer layer.
[0082] The growth pressure of the non-doped GaN layer may be 100-300 Torr. The growth temperature of the non-doped GaN layer may be 100-1200. The present disclosure does not limit this.
[0083] S204: growing an n-type layer on the non-doped GaN layer. The n-type layer includes a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer stacked in sequence, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
[0084] Step S204 can refer to Figure 2 The corresponding description of step S102 is shown in , so it will not be repeated here.
[0085] S205: growing a light-emitting layer on the n-type layer.
[0086] In step S205 , the light emitting layer includes alternately grown InGaN well layers and GaN barrier layers.
[0087] Optionally, the growth temperature and growth pressure of the InGaN well layer are 700-800° C. and 100 torr-300 torr, respectively, and the growth temperature and growth pressure of the GaN barrier layer are 700-900° C. and 100 torr-300 torr, respectively. The quality of the obtained light-emitting layer is good.
[0088] Optionally, the thickness of the InGaN well layer is 2-4 nm, and the thickness of the GaN barrier layer is 5-10 nm. The quality of the obtained light-emitting layer is good.
[0089] S206: growing an AlGaN electron blocking layer on the light emitting layer.
[0090] The growth temperature of the AlGaN electron blocking layer can be 600-1000° C., and the growth pressure of the AlGaN electron blocking layer can be 100-300 Torr. The AlGaN electron blocking layer grown under these conditions has good quality, which is beneficial to improving the luminous efficiency of the light-emitting diode.
[0091] S207: growing a p-type layer on the AlGaN electron blocking layer.
[0092] In step S207 , the p-type layer may be a p-type GaN layer. The growth temperature and growth pressure of the p-type GaN layer may be 850° C. to 1050° C. and 100 Torr to 300 Torr, respectively, so that a p-type layer with better quality can be obtained.
[0093] S208: growing a p-type contact layer on the p-type layer.
[0094] Optionally, the growth pressure of the p-type contact layer may be 100 Torr to 300 Torr, and the growth temperature of the p-type contact layer may be 850° C. to 1050° C.
[0095] In an implementation provided by the present disclosure, the growth temperature of the p-type contact layer may be 950° C., and the growth pressure of the p-type contact layer may be 200 Torr.
[0096] It should be noted that Figure 4 The light emitting diode epitaxial wafer with improved n-type layer and its preparation method shown in Figure 2 The method for preparing a light-emitting diode shown in the figure provides a more detailed growth method of a light-emitting diode epitaxial wafer.
[0097] The structure of the light emitting diode epitaxial wafer after executing step S208 can be seen in Figure 3 .
[0098] It should be noted that in the embodiments of the present disclosure, Veeco K 465i or C4 or RB MOCVD (Metal Organic Chemical Vapor Deposition) equipment is used to realize the growth method of light-emitting diodes. 2 (Hydrogen) or high purity N 2 (nitrogen) or high purity H 2 and high purity N 2 A mixed gas of high purity NH 3 As N source, trimethylgallium (TMGa) and triethylgallium (TEGa) as gallium source, trimethylindium (TMIn) as indium source, silane (SiH4) as N-type dopant, trimethylaluminum (TMAl) as aluminum source, bis(cyclopentadienyl)magnesium (CP 2 Mg) as a P-type dopant.
[0099] The above description does not limit the present disclosure in any form. Although the present disclosure has been disclosed as above through the embodiments, it is not used to limit the present disclosure. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present disclosure. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present disclosure without departing from the content of the technical solution of the present disclosure still falls within the scope of the technical solution of the present disclosure.
Claims
1. A light emitting diode epitaxial wafer with improved n-type layer, characterized in that: The light-emitting diode epitaxial wafer with improved n-type layer comprises a substrate and a non-doped GaN layer, an n-type layer, a light-emitting layer and a p-type layer sequentially stacked on the substrate. The n-type layer includes a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer stacked in sequence, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
2. The light emitting diode epitaxial wafer with improved n-type layer according to claim 1, characterized in that: The doping concentration of silicon in the first silicon-doped gallium nitride sublayer is 0.9-1.5 10 19 cm -3 The doping concentration of silicon in the second silicon-doped gallium nitride sublayer is 1.5 to 4 10 19 cm -3 .
3. The light emitting diode epitaxial wafer with improved n-type layer according to claim 1, characterized in that: The thickness of the first aluminum gallium nitride sublayer is smaller than the thickness of the second aluminum gallium nitride sublayer, and the thickness of the first silicon-doped gallium nitride sublayer is smaller than the thickness of the second silicon-doped gallium nitride sublayer.
4. The light emitting diode epitaxial wafer with improved n-type layer according to any one of claims 1 to 3, characterized in that: The ratio of the thickness of the first aluminum gallium nitride sublayer to the thickness of the second aluminum gallium nitride sublayer is 1:8-1:15, and the ratio of the thickness of the first silicon-doped gallium nitride sublayer to the thickness of the second silicon-doped gallium nitride sublayer is 1:100-1:
120.
5. The light emitting diode epitaxial wafer with improved n-type layer according to any one of claims 1 to 3, characterized in that: The thickness of the first gallium nitride sublayer is 18 nm to 300 nm.
6. A method for preparing a light emitting diode epitaxial wafer with an improved n-type layer, characterized in that: The method for preparing a light emitting diode epitaxial wafer with an improved n-type layer comprises: providing a substrate; An undoped GaN layer, an n-type layer, a light-emitting layer and a p-type layer are sequentially grown on the substrate, the n-type layer comprises a first aluminum gallium nitride sublayer, a first gallium nitride sublayer, a first silicon-doped gallium nitride sublayer, a second silicon-doped gallium nitride sublayer and a second aluminum gallium nitride sublayer which are sequentially stacked, the doping concentration of silicon in the first silicon-doped gallium nitride sublayer is lower than the doping concentration of silicon in the second silicon-doped gallium nitride sublayer, and the Al component in the first aluminum gallium nitride sublayer is higher than the Al component in the second aluminum gallium nitride sublayer.
7. The method for preparing a light emitting diode epitaxial wafer with an improved n-type layer according to claim 6, characterized in that: The n-type layer is grown in an atmosphere of a mixture of hydrogen, ammonia and nitrogen. The volume ratio of hydrogen to ammonia in the atmosphere in which the first silicon-doped gallium nitride sublayer is grown is 2:
1. The volume ratio of hydrogen to ammonia in the atmosphere in which the first aluminum gallium nitride sublayer, the first silicon-doped gallium nitride sublayer, the second silicon-doped gallium nitride sublayer and the second aluminum gallium nitride sublayer are all 3:
2.
8. The method for preparing a light emitting diode epitaxial wafer with an improved n-type layer according to claim 7, characterized in that: The percentage of nitrogen in the atmosphere environment in which the first silicon-doped gallium nitride sublayer is grown is 15%.